Iron atom catalyst with adjustable atomic distance as well as preparation method and application of iron atom catalyst
By preparing iron atomic catalysts with adjustable atomic spacing, the non-radical pathways in the PMS system were regulated, and the problem of difficult catalytic mechanism caused by the randomness of the site structure of iron-based catalysts in the prior art was solved, and antibiotics in complex water quality were achieved Efficient removal of pollutants has wide application prospects and stability.
Patent Information
- Application Number
- CN202411014251.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-26
AI Technical Summary
The random site structure of existing iron-based single-atom catalysts leads to the difficulty in regulating the catalytic mechanism of permonosulfate (PMS), making it difficult to efficiently remove antibiotic pollutants in complex water quality, and the effect of conventional water treatment processes on antibiotic removal is poor .
By preparing an iron atomic catalyst with adjustable atomic spacing, organic molecules with different amino spacings combine with iron ions, combined with Lewis' hard-soft acid and base theory, the non-radical pathway in the PMS system can be regulated to achieve efficient degradation of antibiotics. The catalyst is prepared by mixing iron nitrate nitrate nitrate with aniline ligand, and is prepared by drying, dehydrating, pyrolysis and pickling. It has the ability to remove it to adapt to complex water quality conditions.
It has achieved efficient degradation of antibiotic pollutants in complex water quality, with a removal rate of more than 90%, and has a wide range of pH application and strong stability. It is suitable for industrial production, reducing the environmental hazards of metal ion leaching.
Smart Images

Figure CN118949986A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sewage treatment, and specifically relates to an iron atom catalyst with adjustable atomic spacing, a preparation method and application thereof. Background Art
[0002] Due to the abuse of antibiotics in the medical and aquaculture industries, a large number of antibiotics are left over and discharged into the water environment due to their low biological metabolism rate. Due to the characteristics of antibiotics such as poor biodegradability and bioaccumulation, resistant bacteria and resistance genes in the water environment are increasing, threatening human health and the ecological environment. At the same time, the interference of complex water quality components in wastewater makes conventional water treatment processes face severe challenges in removing antibiotics. Therefore, it is critical to develop water purification technologies that are efficient, economical, safe, stable, and resistant to environmental interference.
[0003] Peroxymonosulfate-based advanced oxidation processes (PMS-AOPs) have significant advantages in removing refractory organic pollutants. On the one hand, PMS can be activated by catalysts to produce hydroxyl radicals ( · OH) and sulfate radicals (SO 4 ·- ), thereby efficiently oxidizing and degrading pollutants. On the other hand, PMS can also be activated by catalysts including singlet oxygen ( 1 O 2 ), high-valent metal oxygen species (HV-Me) and electron transfer, thereby selectively degrading electron-rich recalcitrant organic pollutants, while having strong resistance to environmental interference. Selectively initiating non-radical pathways is expected to play an important role in removing antibiotic pollutants under complex water conditions, which is highly dependent on the site characteristics of the catalyst.
[0004] Single atom catalysts (SACs) with unsaturated metal-Nx sites (M-Nx, where x is the nitrogen coordination number of the metal center) have adjustable site structures, which are conducive to the activation of PMS to initiate non-radical pathways. Among them, iron-based SACs are green, safe, and inexpensive, and have good binding ability and electronic interaction with PMS molecules. However, limited by existing synthesis methods, the site structure of iron-based SACs has a certain randomness, which is not conducive to regulating its catalysis of PMS and the initiation of the mechanism. Therefore, a site-controllable single atom catalyst is urgently needed. Summary of the invention
[0005] In view of this, the purpose of the present invention is to provide an iron atom catalyst with adjustable atomic spacing, a preparation method and application thereof, wherein the obtained catalyst realizes efficient degradation of antibiotics through the combined action of multiple non-radical pathways; it is not easily affected by water quality characteristics, has a wide pH application range, is suitable for the treatment of difficult-to-degrade organic pollutants under complex water quality conditions, and the preparation method is simple and suitable for industrial production.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] In a first aspect, the present invention provides a method for preparing an iron atom catalyst with adjustable atomic spacing, comprising the following steps:
[0008] 1) mixing and dissolving ferric nitrate nonahydrate and aniline ligand, then adding zeolite imidazole framework-8, mixing and drying to obtain an iron atom catalyst precursor;
[0009] 2) The iron atom catalyst precursor is subjected to pyrolysis, acid washing, drying and dehydration in sequence to obtain an iron atom catalyst.
[0010] According to Lewis' hard-soft acid-base theory, amino groups tend to form ionic bonds with hard Lewis acidic metals. Therefore, a molecular recognition strategy is adopted to use organic molecules with different amino group spacings to bind iron ions to assist in forming iron atom catalysts with adjustable spacings, thereby efficiently removing antibiotic pollutants in complex water by regulating the non-free radical pathway in the PMS system.
[0011] Preferably, the preparation method of zeolite imidazole framework-8 in step 1) is: dissolving 2-methylimidazole and zinc nitrate hexahydrate in methanol respectively, then mixing the two solutions and sequentially standing, centrifuging, washing, and drying to obtain zeolite imidazole framework-8.
[0012] Preferably, the molar ratio of the 2-methylimidazole to zinc nitrate hexahydrate is 1:4.
[0013] Preferably, the mixing time is 5 to 10 minutes, the standing time is 12 to 24 hours, the centrifugal speed is 8000 to 10000 r / min, and the washing solvent is methanol.
[0014] Preferably, in step 1), the molar ratio of ferric nitrate nonahydrate to the aniline ligand is 1:3.
[0015] Preferably, the aniline ligand is any one of o-phenylenediamine, p-phenylenediamine or diphenylamine.
[0016] By adopting the above technical solution, different aniline ligands are used to achieve adjustable atomic spacing, where the spacing between the amino groups of o-phenylenediamine is approximately The distance between the amino groups of p-phenylenediamine is approximately The iron atom catalyst with a close atomic distance obtained by using o-phenylenediamine as a ligand initiates a non-radical pathway dominated by HV-Me; the iron atom catalyst with a medium atomic distance obtained by using p-phenylenediamine as a ligand initiates a non-radical pathway dominated by HV-Me. 1 O 2 The non-radical pathway mixed with HV-Me; the iron atom catalyst with a long atomic distance obtained by using diphenylamine as ligand initiated the reaction with 1 O 2 and non-radical pathways dominated by HV-Me, and free radical pathways dominated by ·OH.
[0017] Preferably, the solvent in step 1) is methanol.
[0018] Preferably, in the step 1), the mixing time of the ferric nitrate nonahydrate and the aniline ligand is 2 to 3 hours, and the mixing time of the mixed solution and the zeolite imidazole framework-8 is 1 to 2 hours.
[0019] Preferably, in the pyrolysis step in step 2), nitrogen is used as the protective gas, the heating rate is 5-10° C. / min, the pyrolysis temperature is 800-1000° C., and the pyrolysis holding time is 2-3 h.
[0020] Preferably, the pickling solution used in the pickling step 2) is 0.5 to 1 mol / L H 2 SO 4 Solution, pickling time is 2 to 3 hours.
[0021] Preferably, the drying and dehydration temperature in step 2) is 60-80° C., and the dehydration time is 12-24 hours.
[0022] In a second aspect, the present invention provides an iron atom catalyst with adjustable atomic spacing, which is prepared by the above-mentioned preparation method.
[0023] In a third aspect, the present invention provides the use of the above-mentioned iron atom catalyst with adjustable atomic distance in activating PMS to remove antibiotics from wastewater, characterized in that the antibiotics include tetracycline, bisphenol A, sulfamethoxazole or benzoic acid.
[0024] Preferably, the dosage of the catalyst is 0.025 g / L to 0.2 g / L, and the concentration of the PMS is 0.5 mmol / L to 3 mmol / L.
[0025] Preferably, the pH value of the reaction system for removing antibiotics from wastewater is 1-13, and the temperature of the reaction system is 25-30°C.
[0026] Preferably, the quenching agent for removing antibiotics from wastewater includes ethanol, tert-butanol, furfuryl alcohol and methyl phenyl sulfoxide.
[0027] Contains at least the following beneficial technical effects:
[0028] (1) The present invention obtains an iron atom catalyst precursor by mixing and dissolving ferric nitrate nonahydrate and aniline ligand, then adding zeolite imidazole framework-8 and mixing, followed by drying and dehydration; the iron atom catalyst precursor is subjected to pyrolysis, acid washing, and drying and dehydration in sequence to obtain an iron atom catalyst, which is prepared by a one-step calcination method, and the synthesis process flow is simple.
[0029] (2) The present invention uses Lewis hard and soft acid-base theory and molecular recognition strategy to use aniline compounds with different amino group distances as ligands to bind trivalent iron ions, thereby achieving controllable regulation of the distance between iron atoms.
[0030] (3) The catalyst raw materials of the present invention use ferric nitrate nonahydrate as the metal source and zeolite imidazole framework-8 as the base, which has the advantages of wide material sources and low cost.
[0031] (4) The iron atom catalyst prepared by the present invention inherits the larger specific surface area of the zeolite imidazole framework-8 derived carbon, thereby being able to expose more active sites.
[0032] (5) The catalytic effect of the iron atom catalyst prepared by the present invention only slightly decreases after 4 cycles, and it has strong stability and good regeneration, and effectively reduces the environmental damage caused by metal ion leaching.
[0033] (6) The present invention achieves efficient degradation of antibiotics through the combined action of multiple non-free radical pathways, and more than 90% of antibiotics can be removed in 15 to 20 minutes. It is not easily affected by water quality characteristics, has a wide pH range, and is suitable for the treatment of difficult-to-degrade organic pollutants under complex water conditions, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0035] Figure 1 The removal rate of TC by the catalyst activated PMS prepared in Examples 1 to 5 is shown;
[0036] Figure 2 The removal rate of TC by the catalyst activated PMS prepared in Example 1 and Examples 6-7 at different pyrolysis temperatures;
[0037] Figure 3It is a graph showing the removal rate of TC by PMS activated by catalysts with different aniline ligands prepared in Example 1 and Examples 8-9;
[0038] Figure 4 is a transmission electron microscopy image of the catalyst prepared in Example 8;
[0039] Figure 5 is a transmission electron microscopy image of the catalyst prepared in Example 1;
[0040] Figure 6 is a transmission electron microscopy image of the catalyst prepared in Example 9;
[0041] Figure 7 X-ray diffraction patterns of the catalysts prepared in Example 1 and Examples 8 to 9;
[0042] Figure 8 A spherical aberration-corrected high-angle annular dark-field scanning transmission electron micrograph of the catalyst prepared in Example 8;
[0043] Fig. 9 A spherical aberration-corrected high-angle annular dark-field scanning transmission electron micrograph of the catalyst prepared in Example 1;
[0044] Fig.10 A spherical aberration-corrected high-angle annular dark-field scanning transmission electron micrograph of the catalyst prepared in Example 9;
[0045] Fig.11 It is the adsorption-desorption isotherm diagram of the catalyst prepared in Example 1 and Examples 8-9;
[0046] Fig.12 This is a graph showing the effect of catalyst dosage on the activation of PMS by the catalyst prepared in Example 1 to remove TC;
[0047] Fig.13 This is a graph showing the effect of PMS concentration on the activation of the catalyst prepared in Example 1 to remove TC by PMS;
[0048] Fig.14 This is a graph showing the effect of the initial pH value of the reaction system on the activation of PMS by the catalyst prepared in Example 1 to remove TC;
[0049] Fig.15 This is a graph showing the removal rate of different pollutants by the catalyst activated PMS prepared in Example 8;
[0050] Fig.16 This is a graph showing the removal rate of different pollutants by the catalyst activated PMS prepared in Example 1;
[0051] Fig.17 This is a graph showing the removal rate of different pollutants by the catalyst activated PMS prepared in Example 9;
[0052] Fig.18 This is a graph showing the removal rate of TC by PMS after the catalyst prepared in Example 8 was recycled 4 times and re-fired to activate the catalyst;
[0053] Fig.19 This is a graph showing the removal rate of TC by PMS after the catalyst prepared in Example 1 was recycled 4 times and re-fired to activate the catalyst;
[0054] Fig. 20 This is a graph showing the removal rate of TC by PMS after the catalyst prepared in Example 9 was recycled 4 times and re-fired to activate the catalyst;
[0055] Fig.21 This is a quenching experiment diagram of the catalyst prepared in Example 8 to activate PMS to remove TC;
[0056] Fig. 22 This is a quenching experiment diagram of the catalyst prepared in Example 1 to activate PMS to remove TC;
[0057] Fig.23 This is a quenching experiment diagram of the catalyst prepared in Example 9 to activate PMS to remove TC. DETAILED DESCRIPTION
[0058] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0059] The term "include" or "comprising" in the present invention is an open description containing the specified components or steps described, and other specified components or steps that will not be substantially affected.
[0060] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0061] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased through regular channels.
[0062] Example 1
[0063] This embodiment provides an iron atom catalyst with adjustable atomic spacing, and the preparation steps are as follows:
[0064] 1) Under magnetic stirring conditions, 5.95 g of 2-methylimidazole and 6.57 g of zinc nitrate hexahydrate were dissolved in 150 mL of methanol at a molar ratio of 1:4 to obtain solution A and solution B; then solution A was poured into solution B, mixed and stirred for 5 minutes, and then allowed to stand for 24 hours; the obtained white solid product was centrifuged and washed with methanol 3 times, and dried to obtain zeolite imidazole framework-8;
[0065] 2) Under magnetic stirring conditions, 0.008 g of ferric nitrate nonahydrate and 0.065 g of p-phenylenediamine were mixed and dissolved in 10 mL of methanol in a molar ratio of 1:3, and stirred for 3 h. Then, 0.2 g of zeolite imidazole framework-8 was added thereto, and the mixture was mixed and stirred for 1 h. The mixed product was dried and dehydrated to obtain an iron atom catalyst precursor;
[0066] 3) The iron atom catalyst precursor was placed in a quartz boat and then transferred to a tube furnace. Nitrogen was introduced into the tube furnace to exhaust the air. Then, the temperature was raised to 900°C at a heating rate of 5°C / min and maintained for 2 hours in a nitrogen atmosphere for pyrolysis. After cooling to room temperature, the pyrolysis product was heated in a 1 mol / L H 2 SO 4 After leaching in medium acid for 2 hours and drying and dehydration, the iron atom catalyst FeNC-D-0.02-900 with medium atomic spacing was finally obtained.
[0067] Example 2
[0068] The preparation method of this embodiment is the same as that of embodiment 1, except that ferric nitrate nonahydrate is not added to obtain NC-D.
[0069] Example 3
[0070] The preparation method of this embodiment is the same as that of embodiment 1, except that ferric nitrate nonahydrate and p-phenylenediamine are not added to obtain NC.
[0071] Example 4
[0072] The preparation method of this embodiment is the same as that of embodiment 1, except that the amount of ferric nitrate nonahydrate is 0.01 mmol, i.e., 0.004 g, and the amount of o-phenylenediamine is 0.03 mmol, i.e., 0.033 g, to obtain FeNC-D-0.01-900.
[0073] Example 5
[0074] The preparation method of this embodiment is the same as that of embodiment 1, except that the amount of ferric nitrate nonahydrate is 0.03 mmol, i.e., 0.012 g, and the amount of o-phenylenediamine is 0.09 mmol, i.e., 0.099 g, to obtain FeNC-D-0.03-900.
[0075] Experimental Example 1
[0076] The removal rate of tetracycline (TC) in water by the products of test examples 1 to 5 was tested by the following test method:
[0077] A 250 mL conical flask was selected as the reaction flask, and 100 mL of simulated organic sewage with an initial TC concentration of 10 mg / L was prepared. The pH of the sewage was not adjusted (the pH of the sewage was 6.3 at this time), and 0.05 g / L of the catalyst prepared in Examples 1 to 5 and 1 mmol / L of PMS were added to the reaction flask, respectively. The reaction was carried out by stirring in a constant temperature shaking shaker at 180 r / min at 25°C. The residual concentration of TC was measured at 1 min, 3 min, 5 min, 7 min, 10 min, 15 min, and 20 min of the reaction, and the removal rate of TC was calculated.
[0078] The calculation results are as follows Figure 1 As shown. Figure 1 It can be seen that the removal rate of TC by NC and NC-D alone is low. After the addition of Fe, the removal rate shows a significant improvement, and the TC removal rate reaches more than 90% after 20 minutes of reaction. In addition, with the increase of the proportion of iron, the removal rate of TC shows a trend of first increasing and then decreasing.
[0079] Example 6
[0080] The preparation method of this embodiment is the same as that of embodiment 1, except that the temperature of the tube furnace is raised to 800° C. to obtain FeNC-D-0.2-800.
[0081] Example 7
[0082] The preparation method of this embodiment is the same as that of embodiment 1, except that the temperature of the tube furnace is raised to 1000° C. to obtain FeNC-D-0.2-1000.
[0083] Experimental Example 2
[0084] The removal rate of TC in water by the products of Example 1 and Examples 6-7 was tested, and the testing method was as follows:
[0085] A 250 mL conical flask was selected as the reaction flask, and 100 mL of simulated organic sewage with an initial TC concentration of 10 mg / L was prepared. The pH of the sewage was not adjusted (the pH of the sewage was 6.3 at this time), and 0.05 g / L of the catalyst prepared in Example 1 and Examples 6 to 7 and 1 mmol / L of PMS were added to the reaction flask, respectively. The reaction was carried out by stirring in a constant temperature shaking shaker at 180 r / min at 25°C. The residual concentration of TC was measured at 1 min, 3 min, 5 min, 7 min, 10 min, 15 min, and 20 min of the reaction, and the removal rate of TC was calculated.
[0086] The calculation results are as follows Figure 2 As shown. Figure 2 It can be seen that with the increase of pyrolysis temperature, the removal rate of TC increased significantly, reaching more than 90% at 900°C. As the pyrolysis temperature further increased to 1000°C, the degradation efficiency did not increase significantly.
[0087] Example 8
[0088] The preparation method of this example is the same as that of Example 1, except that the aniline ligand used is o-phenylenediamine, and FeNC-L-0.2-900 is obtained.
[0089] Example 9
[0090] The preparation method of this embodiment is the same as that of embodiment 1, except that the aniline ligand used is diphenylamine, and FeNC-R-0.2-900 is prepared.
[0091] Experimental Example 3
[0092] The removal rate of TC in water by the products of Example 1 and Examples 8 to 9 was tested, and the testing method was as follows:
[0093] A 250 mL conical flask was selected as the reaction flask, and 100 mL of simulated organic sewage with an initial TC concentration of 10 mg / L was prepared. The pH of the sewage was not adjusted (the pH of the sewage was 6.3 at this time), and 0.05 g / L of the catalyst prepared in Example 1 and Examples 8 to 9 and 1 mmol / L of PMS were added to the reaction flask, respectively. The reaction was carried out by stirring in a constant temperature shaking shaker at 180 r / min at 25°C. The residual concentration of TC was measured at 1 min, 3 min, 5 min, 7 min, 10 min, 15 min, and 20 min of the reaction, and the removal rate of TC was calculated.
[0094] The calculation results are as follows Figure 3 As shown. Figure 3 It can be seen that as the distance between Fe atoms increases, the removal rate of TC increases, reaching a maximum removal rate of more than 90% when the atomic distance is medium. As the distance further increases, the TC degradation efficiency decreases.
[0095] Figures 4 to 6 1 is a transmission electron microscope image of the iron atom catalyst prepared in Example 1 and Examples 8 to 9. As shown in the figure, the catalysts are all in a sheet-like structure without obvious iron nanoparticles. The X-ray diffraction images of the iron atom catalysts prepared in Example 1 and Examples 8 to 9 are shown in FIG. Figure 7 As shown in the figure, the catalyst exhibits obvious characteristic peaks at 25° and 44°, corresponding to the (002) and (101) crystal planes of carbon, respectively, and no peaks related to iron-based species appear. Figure 8 to Figure 10 The spherical aberration-corrected high-angle annular dark-field scanning transmission electron micrograph of the iron atom catalyst prepared in Example 1 and Examples 8 to 9, wherein Figure 8 It can be seen that the iron atoms in the catalyst FeNC-L-0.2-900 prepared in Example 8 are distributed in pairs on the surface of the carbon substrate at a closer distance without obvious clusters; Fig. 9 It can be seen that the iron atoms in the catalyst FeNC-D-0.2-900 prepared in Example 1 are distributed in pairs on the surface of the carbon substrate at a medium distance without obvious clusters. Fig.10 It can be seen that the iron atoms in the catalyst FeNC-R-0.2-900 prepared in Example 9 are independently and evenly distributed on the surface of the carbon substrate, with a large distance between them and no obvious clusters. Fig.11 The adsorption-desorption isotherms of the iron atom catalysts prepared in Example 1 and Examples 8 to 9 show that the prepared catalysts have a large specific surface area.
[0096] Example 10
[0097] This embodiment provides an iron atom catalyst with adjustable atomic spacing, and the preparation steps are as follows:
[0098] 1) Under magnetic stirring conditions, 5.95 g of 2-methylimidazole and 6.57 g of zinc nitrate hexahydrate were dissolved in 150 mL of methanol at a molar ratio of 1:4 to obtain solution A and solution B; then solution A was poured into solution B, mixed and stirred for 10 min, and then allowed to stand for 12 h; the obtained white solid product was centrifuged and washed with methanol 3 times, and dried to obtain zeolite imidazole framework-8;
[0099] 2) Under magnetic stirring conditions, 0.008 g of ferric nitrate nonahydrate and 0.065 g of p-phenylenediamine were mixed and dissolved in 10 mL of methanol in a molar ratio of 1:3, and stirred for 2 h. Then, 0.2 g of zeolite imidazole framework-8 was added thereto, and the mixture was mixed and stirred for 2 h. The mixed product was dried and dehydrated to obtain an iron atom catalyst precursor;
[0100] 3) The iron atom catalyst precursor was placed in a quartz boat and then transferred to a tube furnace. Nitrogen was introduced into the tube furnace to exhaust the air. Then, the temperature was raised to 900°C at a heating rate of 10°C / min and maintained for 3 hours in a nitrogen atmosphere for pyrolysis. After cooling to room temperature, the pyrolysis product was heated in a 0.5 mol / L H 2 SO 4 After leaching in medium acid for 3 hours and drying and dehydration, the iron atom catalyst FeNC-D-0.02-900 with medium atomic spacing was finally obtained.
[0101] In this embodiment, the TC removal rate reaches more than 90%.
[0102] Experimental Example 4
[0103] Four treatment groups were set up with the iron atom catalyst prepared in Example 1: a 250 mL conical flask was selected as the reaction bottle, and 100 mL of simulated organic sewage with an initial TC concentration of 10 mg / L was prepared. The pH of the sewage was not adjusted (the pH of the sewage was 6.3 at this time), and 0.025 g / L (treatment group 1), 0.05 g / L (treatment group 2), 0.1 g / L (treatment group 3), 0.2 g / L (treatment group 4) of catalyst and 1 mmol / L of PMS were added to the four reaction systems, respectively. The mixture was fully stirred in a constant temperature shaking shaker at 180 r / min at 25-30°C for reaction. The residual concentration of TC was measured at 1 min, 3 min, 5 min, 7 min, 10 min, 15 min, and 20 min of reaction, and the removal rate of TC was calculated.
[0104] The calculation results are as follows Fig.12 As shown. Fig.12 It can be seen that as the catalyst dosage increases from 0.025g / L to 0.05g / L, the removal rate of DOX increases significantly, reaching a maximum removal rate of more than 90% at 0.05g / L, indicating that as the catalyst dosage increases, the catalyst can provide more active sites during the reaction and produce a large number of active species, thereby improving the TC removal rate. When the catalyst dosage is further increased to 0.2g / L, the removal rate of TC only increases slightly, indicating that the active sites provided by the catalyst are excessive and cannot be fully utilized during the reaction. The above analysis results show that in practical applications, the catalyst dosage can be adjusted according to the actual situation of local sewage and the requirements of treatment efficiency, so as to achieve the purpose of efficient removal of organic pollutants.
[0105] Experimental Example 5
[0106] Four treatment groups were set up with the iron atom catalyst prepared in Example 1: a 250 mL conical flask was selected as the reaction bottle, and 100 mL of simulated organic sewage with an initial TC concentration of 10 mg / L was prepared. The pH of the sewage was not adjusted (the pH of the sewage was 6.3 at this time), and PMS 0.5 mmol / L (treatment group 1), 1.0 mmol / L (treatment group 2), 2.0 mmol / L (treatment group 3), 3.0 mmol / L (treatment group 4) and 0.3 g / L of the catalyst were added to the four reaction systems, respectively. The mixture was fully stirred in a constant temperature shaking shaker at 180 r / min at 25-30° C. for reaction. The residual concentration of TC was measured at 1 min, 3 min, 5 min, 7 min, 10 min, 15 min, and 20 min of the reaction, and the removal rate of TC was calculated.
[0107] The calculation results are as follows Fig.13 As shown. Fig.13 It can be seen that with the increase of PMS concentration, the removal rate of TC continues to increase and can reach a high level, indicating that in practical applications, the concentration of PMS can be adjusted according to the actual situation of local sewage and the requirements of treatment efficiency to achieve the purpose of controlling costs and improving removal efficiency.
[0108] Experimental Example 6
[0109] Seven treatment groups were set up with the iron atom catalyst prepared in Example 1: a 250 mL conical flask was selected as the reaction flask, and 100 mL of simulated organic sewage with an initial TC concentration of 10 mg / L was prepared. The initial pH of the sewage was adjusted to: 1 (treatment group 1), 3 (treatment group 2), 5 (treatment group 3), 7 (treatment group 4), 9 (treatment group 5), 11 (treatment group 6), and 13 (treatment group 7), respectively. 0.05 g / L of catalyst and 1 mmol / L of PMS were added to the reaction flasks, respectively. The mixture was fully stirred in a constant temperature shaking shaker at 180 r / min at 25-30°C for reaction. The residual concentration of TC was measured at 1 min, 3 min, 5 min, 7 min, 10 min, 15 min, and 20 min of the reaction, and the removal rate of TC was calculated.
[0110] The calculation results are as follows Fig.14 As shown. Fig.14 It can be seen that, except for pH values of 1 and 13, the TC removal rate reached more than 90% under other pH conditions, indicating that in practical applications, the system has strong adaptability to the pH values of sewage under different environments and can efficiently treat antibiotics in various types of sewage.
[0111] Experimental Example 7
[0112] Four treatment groups were set up with the iron atom catalyst prepared in Example 1 and Examples 8 to 9: a 250 mL conical flask was used as a reaction flask, and 100 mL of simulated organic sewage containing different pollutants with an initial concentration of 10 mg / L was prepared respectively: bisphenol A (BPA, treatment group 1), TC (treatment group 2), sulfamethoxazole (SMX, treatment group 3), benzoic acid (BA, treatment group 4), without adjusting the pH of the sewage (the pH of the sewage was 6.3 at this time), 0.05 g / L of catalyst and 1 mmol / L of PMS were added to the reaction flasks, and the mixture was fully stirred in a constant temperature shaking shaker at 180 r / min at 25 to 30° C. for reaction, and the residual concentration of TC was measured at 1 min, 3 min, 5 min, 7 min, 10 min, 15 min, and 20 min of the reaction, and the removal rate of TC was calculated.
[0113] The calculation results are as follows Figure 15 to Figure 17 The degradation of different pollutants in the three systems showed obvious differences. Fig.15 It can be seen that the catalyst prepared in Example 1 can achieve a removal rate of more than 80% for pollutants with low ionization potential (BPA, TC, SMX) within 20 minutes, but it is difficult to effectively degrade pollutants with high ionization potential (BA), indicating that the oxidation pathway of pollutants in this system is a non-radical pathway that can selectively degrade pollutants with low ionization potential; Fig.16 It can be seen that the catalyst prepared in Example 8 can achieve a removal rate of more than 90% for pollutants with low ionization potential (BPA, TC, SMX) within 20 minutes, but it is difficult to effectively degrade pollutants with high ionization potential (BA), indicating that the oxidation pathway of pollutants in this system is a non-radical pathway that can selectively degrade pollutants with low ionization potential; Fig.17 It can be seen that the catalyst prepared in Example 9 can achieve a removal rate of more than 60% for pollutants with low ionization potential (BPA, TC, SMX) within 20 minutes, while the removal rate for pollutants with high ionization potential (BA) is only about 30%, indicating that the oxidation pathway of pollutants in this system is mainly non-radical pathways that can selectively degrade low ionization potential pollutants, in addition, the free radical pathway also makes a weak contribution.
[0114] Experimental Example 8
[0115] The cyclic stability of the catalyst was tested with the iron atom catalyst prepared in Example 1 and Examples 8-9: a 250 mL conical flask was used as the reaction flask, 100 mL of simulated organic sewage with an initial TC concentration of 10 mg / L was prepared, the pH of the sewage was not adjusted (the pH of the sewage was 6.3 at this time), 0.05 g / L of catalyst and 1 mmol / L of PMS were added to the reaction system, and the reaction was fully stirred in a constant temperature shaking shaker at 180 r / min at 25-30 ° C. The residual concentration of TC was measured at 1 min, 3 min, 5 min, 7 min, 10 min, 15 min, and 20 min of the reaction, and the removal rate of TC was calculated. After the reaction was completed, the degraded catalyst was collected by suction filtration, washed with deionized water, filtered and dried, and a cyclic experiment was carried out according to the above test method.
[0116] Test results such as Figure 18 to Figure 20 As shown. Fig.18 It can be seen that after five cycles, the degradation rate of TC by the catalyst prepared in Example 8 decreased by 27.4%, and recovered to 85.6% after re-firing at 350°C, indicating that the active sites have strong regeneration properties. Fig.19 It can be seen that the degradation rate of TC by the catalyst prepared in Example 1 decreased by 12.3%, and recovered to 90.4% after re-firing at 350°C, indicating that the active sites have stronger regeneration properties. Fig. 20 It can be seen that the degradation rate of TC by the catalyst prepared in Example 9 decreased by 27.7%, and recovered to 57.5% after re-firing at 350° C., indicating that the active sites are not easy to regenerate.
[0117] Experimental Example 9
[0118] Four treatment groups and one untreated group were set up with the iron atom catalyst prepared in Example 1 and Examples 8 to 9 for quenching experiments: a 250 mL conical flask was selected as a reaction flask, 100 mL of simulated organic sewage with an initial TC concentration of 10 mg / L was prepared, the pH of the sewage was not adjusted (the pH of the sewage was 6.0 at this time), 0.05 g / L of catalyst and 1 mmol / L of PMS were added to the reaction flask, and 1000 mmol / L of ethanol (EtOH) was added as a quencher of sulfate radicals and hydroxyl radicals (treatment group 1), 1000 mmol / L of ethanol (EtOH) was added as a quencher of sulfate radicals and hydroxyl radicals (treatment group 2), and 1000 mmol / L of ethanol (EtOH) was added as a quencher of sulfate radicals and hydroxyl radicals (treatment group 3). 50 mmol / L tert-butyl alcohol (TBA) was used as a quencher of hydroxyl radicals (treatment group 2), 50 mmol / L furfuryl alcohol (FFA) was used as a quencher of singlet oxygen (treatment group 3), and 50 mmol / L methyl phenyl sulfoxide (PMSO) was used as a quencher of high-valent iron species (treatment group 4). The mixture was fully stirred in a constant temperature shaking incubator at 180 r / min for reaction. The residual concentration of TC was determined at 1 min, 3 min, 5 min, 7 min, 10 min, 15 min, and 20 min of reaction, and the removal rate of TC was calculated.
[0119] The calculation results are as follows Figure 21 to Figure 23 As shown. Fig.21 It can be seen that in the catalyst system prepared in Example 1, after adding ethanol and tert-butyl alcohol, the inhibitory effect on TC removal is negligible, indicating that SO 4 ·- and · OH plays a minor role in the reaction process; after adding furfuryl alcohol, the removal of TC was only inhibited by 8.34%, indicating that 1 O 2 It plays a minor role in the reaction process; after adding methyl phenyl sulfoxide, the removal of TC was inhibited by 72.31%, indicating that the non-free radical pathway dominated by HV-Me plays the most important role in the removal of TC. Fig. 22 It can be seen that in the catalyst system prepared in Example 8, after adding ethanol and tert-butyl alcohol, the inhibitory effect on TC removal is negligible, indicating that SO 4 ·- and · OH played a minor role in the reaction process; after adding furfuryl alcohol and methyl phenyl sulfoxide, the removal of TC was inhibited by 27.06% and 53.42%, respectively, indicating that HV-Me was the main 1 O 2 The non-radical pathway plays a major role in TC removal, with the auxiliary pathway being Fig.23 It can be seen that in the catalyst system prepared in Example 9, after adding ethanol and tert-butyl alcohol, the inhibition rates of TC removal were 20.21% and 17.21% respectively, indicating that · OH plays a weak role in the reaction process, SO 4 ·- The role played in the reaction process can be ignored; after adding furfuryl alcohol and methyl phenyl sulfoxide, the removal of TC was inhibited by 43.83% and 13.36%, respectively. 1 O 2 The non-radical pathway mainly with HV-Me as the auxiliary plays the most important role in TC removal. · The OH-based free radical pathway also made a slight contribution. The non-free radical pathway is less affected by changes in external conditions and can treat antibiotic pollutants in complex water quality in a variety of situations.
[0120] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A method for preparing an iron atom catalyst with adjustable atomic spacing, characterized in that: The following steps are involved: 1) mixing and dissolving ferric nitrate nonahydrate and aniline ligand, then adding zeolite imidazole framework-8, mixing and drying to obtain an iron atom catalyst precursor; 2) The iron atom catalyst precursor is subjected to pyrolysis, acid washing, drying and dehydration in sequence to obtain an iron atom catalyst.
2. The preparation method according to claim 1, characterized in that: The preparation method of zeolite imidazole framework-8 in step 1) is: dissolving 2-methylimidazole and zinc nitrate hexahydrate in methanol respectively, then mixing the two solutions and sequentially standing, centrifuging, washing, and drying to obtain zeolite imidazole framework-8.
3. The preparation method according to claim 2, characterized in that: The molar ratio of the 2-methylimidazole to zinc nitrate hexahydrate is 1:
4.
4. The preparation method according to claim 1, characterized in that: In the step 1), the molar ratio of ferric nitrate nonahydrate to aniline ligand is 1:3; The aniline ligand is any one of o-phenylenediamine, p-phenylenediamine or diphenylamine.
5. The preparation method according to claim 1, characterized in that: In the step 1), the mixing time of ferric nitrate nonahydrate and aniline ligand is 2 to 3 hours, and the mixing time of the mixed solution and zeolite imidazole framework-8 is 1 to 2 hours.
6. The preparation method according to claim 1, characterized in that: In the pyrolysis step in step 2), nitrogen is used as the protective gas, the heating rate is 5-10°C / min, the pyrolysis temperature is 800-1000°C, and the pyrolysis holding time is 2-3h; The pickling solution used in the step 2) is a 0.5-1 mol / L H2SO4 solution, and the pickling time is 2-3 hours.
7. An iron atom catalyst with adjustable atomic spacing, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 6.
8. Use of the iron atom catalyst with adjustable atomic distance as claimed in claim 7 in activating PMS to remove antibiotics from wastewater, characterized in that: The antibiotics include tetracycline, bisphenol A, sulfamethoxazole or benzoic acid.
9. The use according to claim 8, characterized in that: The dosage of the catalyst is 0.025 g / L to 0.2 g / L, and the concentration of the PMS is 0.5 mmol / L to 3 mmol / L.
10. The use according to claim 8, characterized in that: The pH value of the reaction system for removing antibiotics from wastewater is 1-13, and the temperature of the reaction system is 25-30°C.
Citation Information
Patent Citations
Non-pgm cathode catalysts for fuel cell application derived from heat treated heteroatomic amines precursors
CN103998131A
Preparation method of FeNi-N / Al2O3 / C catalyst, catalyst and application thereof
CN106362786A
Iron-based carbon-nitrogen compound catalytic material for efficiently treating organic wastewater and preparation method thereof
CN111346661A
Preparation method of single-atom iron-based oxygen reduction catalyst
CN111952608A
Iron monatomic catalyst as well as preparation method and application thereof
CN112495417A