Method for preparing reforming hydrogen production catalyst by taking waste vanadium-titanium denitration catalyst as raw material and application of reforming hydrogen production catalyst
By performing multiple steps on the waste vanadium titanium denitrification catalyst, an efficient Ni-based reforming hydrogen production catalyst was prepared, which solved the problem of poor dispersion of Ni particles, significantly improved the activity and stability of the catalyst, and achieved excellent methane Hydrogen production performance by steam reforming.
Patent Information
- Application Number
- CN202411032300.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-30
AI Technical Summary
In the prior art, Ni-based catalysts have high initial activity in methane reforming hydrogen production reaction, but the Ni particles are poorly dispersed, resulting in the catalyst deactivation, and the used vanadium titanium denitrification catalyst has excellent thermal stability but the active center Ni dispersibility is required. improve.
Porous support is prepared to fully disperse Ni to form efficient Ni reforming and hydrogenation by crushing the used vanadium titanium denitrification catalyst, reducing NaBH4, granulation, hydroxylation, aminolation, carboxy grafting and nickel salt ion exchange. catalyst.
The reforming hydrogen production efficiency of the catalyst and the dispersion of the active center Ni are improved, and the catalytic performance and stability in the reforming hydrogen production by methane water vapor are significantly improved.
Smart Images

Figure CN118949997A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a reforming hydrogen production catalyst using waste vanadium-titanium denitration catalyst as a raw material and application thereof, belonging to the technical field of environmental protection catalysis and new energy. Background Art
[0002] With the rapid development of industrialization, large amounts of nitrogen oxides have been emitted, causing acid rain, photochemical smog, haze and other air pollution problems. Selective oxidation-reduction technology (SCR) has been widely used in the field of denitrification. The catalyst commonly used in the SCR denitrification process is vanadium-titanium denitrification catalyst, which can usually be regenerated 2 to 3 times before it can only be completely scrapped. Therefore, the resource utilization of waste vanadium-titanium denitrification catalyst has become an environmental problem that needs to be solved urgently.
[0003] Hydrogen is an important green new energy source with the advantages of high combustion calorific value; theoretically, water is the only combustion product and it is very clean. Methane reforming is an economical and efficient method of hydrogen production, such as methane steam reforming and methane carbon dioxide reforming. Among them, methane steam reforming is the most widely used and has been industrialized on a large scale. About 10% of the world's hydrogen is produced by this method.
[0004] The carrier plays an extremely important role in the methane reforming hydrogen production catalyst. It not only provides physical support for the metal active components, but also interacts strongly with the active components to affect the performance of the catalyst. Some carriers also directly participate in the reaction. Thermodynamic calculations show that the methane reforming hydrogen production reaction requires high temperatures to obtain a sufficiently high hydrogen yield. Therefore, whether it is steam reforming or dry gas reforming, the catalyst carrier of the reforming reaction must have high thermal stability.
[0005] Ni-based catalysts have high initial activity in methane reforming hydrogen production reactions, but the poor dispersion of Ni particles can easily lead to catalyst deactivation, so the core problem that needs to be solved is to promote the dispersion of the active center Ni in the carrier. Waste vanadium titanium denitrification catalysts contain 70-85% titanium dioxide and have excellent thermal stability, so they can be used as carriers for Ni-based catalysts, but how to further improve the dispersion of the active center Ni in the carrier is still a difficult problem that the existing technology needs to overcome. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing a reforming hydrogen production catalyst using waste vanadium titanium denitration catalyst as a raw material and its application. The waste vanadium titanium denitration catalyst is recycled to prepare a porous carrier, which is then subjected to hydroxyl-enriched treatment, amino modification, carboxyl grafting, ion exchange with a nickel salt, and calcination, so that Ni can be fully dispersed and loaded on the porous carrier, thereby improving its reforming hydrogen production efficiency.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] A method for preparing a reforming hydrogen production catalyst using waste vanadium-titanium denitration catalyst as a raw material comprises the following steps:
[0009] S1. The waste vanadium titanium denitration catalyst is crushed and dispersed in a NaBH4 solution, heated and stirred for reaction, filtered and dried, and the obtained product is then mixed with a forming agent and a pore-forming agent, and then granulated and calcined to obtain a porous carrier;
[0010] S2, mixing the porous carrier and the fluorine-containing ionic liquid, heating, separating, drying and calcining to obtain a hydroxyl-rich porous carrier;
[0011] S3, mixing the hydroxyl-rich porous carrier with an amino-containing silane coupling agent and performing an amination treatment to obtain an amination porous carrier; and then reacting the amination porous carrier with a carboxyl-containing compound to obtain a carboxyl-grafted porous carrier;
[0012] S4. Immerse the porous carrier grafted with carboxyl groups in a nickel salt solution and perform ultrasonic treatment, and then separate, dry and calcine to obtain a Ni-based reforming hydrogen production catalyst.
[0013] Preferably, the waste vanadium titanium denitrification catalyst uses TiO2 as a carrier, V2O5 and WO3 as active components, and the rest are co-catalysts; wherein the TiO2 carrier is 70% to 85% of the content of the waste vanadium titanium denitrification catalyst, and the active components V2O5 and WO3 are 1% to 4% and 1% to 3% of the content of the waste vanadium denitrification catalyst, respectively.
[0014] Preferably, in step S1, the concentration of the NaBH4 solution is 10-15%;
[0015] The mixing ratio of the crushed vanadium titanium denitration catalyst and the NaBH4 solution is (3-5) g: (10-20) ml;
[0016] The conditions for the heating and stirring reaction are: temperature 50-70°C, rotation speed 50-100 rpm, 0.5-1.5h;
[0017] Drying conditions are: 85-120℃, 1-3h.
[0018] Preferably, in step S1, the molding agent is a 1-15wt% poly(ethylene) acid solution;
[0019] The pore-forming agent is a 10-20wt% urea solution;
[0020] The mass ratio of the obtained product to the forming agent and the pore-forming agent is (50-65):(3-10):(2-7);
[0021] The calcination conditions are: 1000-1250°C, 1-2.5h.
[0022] Preferably, in step S2, the fluorine-containing ionic liquid is 1-butyl-3-methylimidazolium tetrafluoroborate ([BMIm][BF4]);
[0023] The mass ratio of the porous carrier to the fluorine-containing ionic liquid is (1-3):(5-8);
[0024] The heating conditions are: 150-200°C, 15-25h;
[0025] The calcination conditions are: 700-900°C, 1-2.5h.
[0026] Preferably, in step S3, the specific preparation method of the aminated porous carrier is:
[0027] The hydroxyl-rich porous carrier, the amino-containing silane coupling agent, and anhydrous ethanol are mixed in a mass ratio of (2-4):1:(10-15), stirred at room temperature for 10-15 minutes, and then allowed to stand for 1-1.5 hours, filtered, and the filter residue is dried at 100-120°C for 1-2 hours;
[0028] Wherein, the amino-containing silane coupling agent is (3-aminopropyl)triethoxysilane.
[0029] Preferably, in step S3, the specific preparation method of the carboxyl-grafted porous carrier is:
[0030] The aminated porous carrier, the carboxyl-containing compound and DMF are mixed in a mass ratio of (2-5):(1-2):(10-20), stirred at room temperature for 15-25 minutes, allowed to stand for 1-2 hours, filtered, and the residue is dried at 110-130°C for 2-3 hours;
[0031] Wherein, the carboxyl-containing compound is succinic anhydride.
[0032] Preferably, in step S4, the nickel salt is NiCl2·6H2O or Ni(NO3)2·6H2O or NiSO4·6H2O;
[0033] The mass ratio of the carboxyl-grafted porous carrier to the nickel salt in the nickel salt solution is (8-12):(1-3).
[0034] Preferably, in step S4, the conditions for ultrasonic treatment are: 20-50kHz, 0.5-1h;
[0035] Drying conditions are: 70-90°C, 1-1.5h;
[0036] The calcination conditions are: 1100-1250°C, 0.5-2h.
[0037] A reforming hydrogen production catalyst is prepared by any of the above methods.
[0038] The reforming hydrogen production catalyst prepared by any of the above methods or the use of the above reforming hydrogen production catalyst in methane steam reforming hydrogen production.
[0039] The beneficial effects of the present invention are:
[0040] The number of oxygen vacancies in the waste vanadium-titanium denitrification catalyst will decrease due to deactivation and other reasons. Therefore, the crushed waste vanadium-titanium denitrification catalyst is first reduced with NaBH4 to increase the number of oxygen vacancies, and then mixed with a forming agent and a pore-forming agent to form a porous carrier by granulation and calcination. During the calcination process, the pore-forming agent will generate gas to break through the powder and form a pore structure, which can then increase the specific surface area of the porous carrier and facilitate the subsequent distribution of nickel.
[0041] The increase in the number of oxygen vacancies is conducive to the hydroxylation of the porous carrier. The fluoride ions in the ammonium fluoride ionic liquid interact with the oxygen vacancies on the surface of titanium dioxide, promoting the adsorption and dissociation of water molecules on the surface. The hydroxyl groups generated after the dissociation of water molecules combine with the surface of titanium dioxide to form a hydroxyl-rich surface structure. After the hydroxylation treatment, the amination treatment and carboxylation grafting are carried out in sequence, and finally the nickel ions are loaded onto the porous carrier by ion exchange. After calcination, a Ni-based reforming hydrogen production catalyst with fully dispersed active centers is obtained. Due to the full dispersion of the active centers, the catalyst exhibits excellent catalytic performance in methane steam reforming hydrogen production. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 is the methane conversion rate of the catalysts obtained in Example 1 and Comparative Examples 1-3;
[0043] Figure 2 The figure is a graph showing the change in methane conversion rate of the catalyst obtained in Example 1 versus reaction time. DETAILED DESCRIPTION
[0044] The present invention will be specifically described below in conjunction with the accompanying drawings and embodiments.
[0045] Example 1
[0046] The waste vanadium titanium denitration catalyst (TiO2 content 80%, V2O5 content 3%, WO3 content 2%) was crushed and screened into 30g of 100-150 mesh fine particles, and then dispersed in 200ml of 15% NaBH4 solution, stirred at 55℃, 100rpm for 1h, and filtered, and the filter residue was dried at 100℃ for 1.5h. 25g of the obtained product was taken, mixed with 5g of 15wt% polyacrylic acid solution and 3g of 20wt% urea solution, granulated, and then calcined at 1100℃ for 2h to obtain a porous carrier.
[0047] Take 20g of the porous carrier and mix it with 50ml of 1-butyl-3-methylimidazolium tetrafluoroborate, 50ml of acetic acid and 50ml of deionized water, treat it at 180℃ for 24h, separate it after treatment, dry it, calcine it at 850℃ for 2h and cool it to room temperature, then mix it with 10g (3-aminopropyl) triethoxysilane and 120g of anhydrous ethanol and stir it for 15min and let it stand for 1.5h, filter it after standing, dry the filter residue at 100℃ for 1h and cool it to room temperature, then mix it with 11g of succinic anhydride and 150g of DMF and stir it for 120min and let it stand for 2h, filter it after standing, and dry the filter residue at 110℃ for 2h to obtain a carboxyl-grafted porous carrier.
[0048] 20 g of the carboxyl-grafted porous support was immersed in 100 ml of an aqueous solution containing 3 g of Ni(NO3)2·6H2O and treated with ultrasound (30 kHz) for 1 h. After separation, it was dried at 75°C for 1.5 h and then calcined at 1100°C for 2 h to obtain a Ni-based reforming hydrogen production catalyst.
[0049] Comparative Example 1
[0050] The method is basically the same as Example 1, except that in Example 1, the crushed waste vanadium-titanium denitration catalyst is not subjected to reduction treatment.
[0051] Specifically:
[0052] The waste vanadium-titanium denitrification catalyst (TiO2 content 80%, V2O5 content 3%, WO3 content 2%) was crushed and screened into 25g of 100-150 mesh fine particles, which were evenly mixed with 5g of 15wt% polyethylene acid solution and 3g of 20wt% urea solution, and then granulated. The mixture was then calcined at 1100°C for 2h to obtain a porous carrier.
[0053] Take 20g of the porous carrier and mix it with 50ml of 1-butyl-3-methylimidazolium tetrafluoroborate, 50ml of acetic acid and 50ml of deionized water, treat it at 180℃ for 24h, separate it after treatment, dry it, calcine it at 850℃ for 2h and cool it to room temperature, then mix it with 10g (3-aminopropyl) triethoxysilane and 120g of anhydrous ethanol and stir it for 15min and let it stand for 1.5h, filter it after standing, dry the filter residue at 100℃ for 1h and cool it to room temperature, then mix it with 11g of succinic anhydride and 150g of DMF and stir it for 120min and let it stand for 2h, filter it after standing, and dry the filter residue at 110℃ for 2h to obtain a carboxyl-grafted porous carrier.
[0054] 20 g of the carboxyl-grafted porous support was immersed in 100 ml of an aqueous solution containing 3 g of Ni(NO3)2·6H2O and treated with ultrasound (30 kHz) for 1 h. After separation, it was dried at 75°C for 1.5 h and then calcined at 1100°C for 2 h to obtain a Ni-based reforming hydrogen production catalyst.
[0055] Comparative Example 2
[0056] The method is basically the same as Example 1, except that in Comparative Example 2, the hydroxyl-rich porous carrier is not subjected to an amination treatment.
[0057] Specifically:
[0058] The waste vanadium titanium denitration catalyst (TiO2 content 80%, V2O5 content 3%, WO3 content 2%) was crushed and screened into 30g of 100-150 mesh fine particles, and then dispersed in 200ml of 15% NaBH4 solution, stirred at 55℃, 100rpm for 1h, and filtered, and the filter residue was dried at 100℃ for 1.5h. 25g of the obtained product was taken, mixed with 5g of 15wt% polyacrylic acid solution and 3g of 20wt% urea solution, granulated, and then calcined at 1100℃ for 2h to obtain a porous carrier.
[0059] Take 20g of the porous carrier and mix it with 50ml of 1-butyl-3-methylimidazolium tetrafluoroborate, 50ml of acetic acid and 50ml of deionized water, treat it at 180℃ for 24h, separate it after treatment, dry it, calcine the product at 850℃ for 2h and cool it to room temperature, then mix it with 11g of succinic anhydride and 150g of DMF and stir it for 120min and let it stand for 2h, filter it after standing, dry the filter residue at 110℃ for 2h and cool it to room temperature, take 20g of the above product and immerse it in 100ml aqueous solution containing 3g of Ni(NO3)2·6H2O and treat it with ultrasound (30kHz) for 1h, dry it at 75℃ for 1.5h after separation, and then calcine it at 1100℃ for 2h to obtain a Ni-based reforming hydrogen production catalyst.
[0060] Comparative Example 3
[0061] The method is basically the same as Example 1, except that in Comparative Example 3, the amino-modified porous carrier is not subjected to carboxyl grafting treatment.
[0062] Specifically:
[0063] The waste vanadium titanium denitration catalyst (TiO2 content 80%, V2O5 content 3%, WO3 content 2%) was crushed and screened into 30g of 100-150 mesh fine particles, and then dispersed in 200ml of 15% NaBH4 solution, stirred at 55℃, 100rpm for 1h, and filtered, and the filter residue was dried at 100℃ for 1.5h. 25g of the obtained product was taken, mixed with 5g of 15wt% polyacrylic acid solution and 3g of 20wt% urea solution, granulated, and then calcined at 1100℃ for 2h to obtain a porous carrier.
[0064] Take 20g of the porous carrier and mix it with 50ml of 1-butyl-3-methylimidazolium tetrafluoroborate, 50ml of acetic acid and 50ml of deionized water, treat it at 180°C for 24h, separate it after the treatment, dry it, calcine it at 850°C for 2h and then cool it to room temperature, then mix it with 10g of (3-aminopropyl) triethoxysilane and 120g of anhydrous ethanol and stir it for 15min and then let it stand for 1.5h. After standing, filter it, dry the filter residue at 100°C for 1h and then cool it to room temperature to obtain an amino porous carrier.
[0065] 20 g of the aminated porous support was immersed in 100 ml of an aqueous solution containing 3 g of Ni(NO3)2·6H2O and treated with ultrasound (30 kHz) for 1 h. After separation, it was dried at 75°C for 1.5 h and then calcined at 1100°C for 2 h to obtain a Ni-based reforming hydrogen production catalyst.
[0066] The atmospheric pressure activity evaluation of methane steam reforming hydrogen production catalyst was carried out in a fixed bed stainless steel tube reactor (ID = 8mm). The catalyst loading was 100mg, and the catalyst was pretreated at 800℃ for 2h in a 10% H2 / Ar atmosphere before the reaction, with a reducing gas of 60mL / min. The reaction raw materials were pure methane (99.99%) and deionized water. The deionized water was first injected into a 200℃ preheating furnace through a high-pressure circulating water pump for vaporization. The injection rate was 0.064mL / min, and 40mL / min of methane gas was introduced. After mixing with the water vapor formed by deionized water, it entered the reactor for reaction. The reaction mass space velocity was 72000mL·h -1 ·gcat -1, the water-carbon ratio is 2:1. After the reaction tail gas is cooled in an ice-water bath, it is fed into a GC9310 gas chromatograph for online analysis. Ar gas (99.9%) is used as the carrier gas, TCD detector, bridge flow is 80 mA, column box temperature is 110°C, the chromatographic column is TDX-01 columnar molecular sieve (2m), and the N2000 chromatographic workstation is used to collect data. The reaction conversion rate is calculated by the area normalization method.
[0067] The catalytic activity of the Ni-based reforming hydrogen production catalyst obtained in Example 1 and Comparative Examples 1-3 at atmospheric pressure reforming at different reaction temperatures is as follows: Figure 1 As shown, the methane conversion rate of the catalyst increases with the increase of temperature, and the Ni-based reforming hydrogen production catalyst obtained in Example 1 shows the best methane conversion rate (99.7%). The reason is that the reduction treatment of NaBH4 can increase the number of oxygen vacancies and facilitate the hydroxylation of the porous carrier. The hydroxylation-rich structure is conducive to the dispersion of amino groups. Therefore, during the carboxylation grafting treatment, (3-aminopropyl)triethoxysilane can combine with the amino groups dispersed on the porous carrier to introduce carboxyl groups into the porous carrier. The dispersion of carboxyl groups can increase the dispersion of nickel ions when nickel ions are loaded onto the porous carrier through ion exchange. Therefore, the active center Ni of the Ni-based reforming hydrogen production catalyst obtained after calcination will be fully dispersed, and it will show excellent catalytic performance in methane steam reforming hydrogen production. And from Figure 2 It can be seen that the activity of the Ni-based reforming hydrogen production catalyst prepared in Example 1 is relatively stable in the 200h stability experiment, without large fluctuations and obvious decline.
[0068] The above is only a preferred implementation of the patent of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the patent of the present invention. These improvements and modifications should also be regarded as the scope of protection of the patent of the present invention.
Claims
1. A method for preparing a reforming hydrogen production catalyst using waste vanadium-titanium denitration catalyst as raw material, characterized in that: The steps include: S1. The waste vanadium titanium denitration catalyst is crushed and dispersed in a NaBH4 solution, heated and stirred for reaction, filtered and dried, and the obtained product is then mixed with a forming agent and a pore-forming agent, and then granulated and calcined to obtain a porous carrier; S2, mixing the porous carrier and the fluorine-containing ionic liquid, heating, separating, drying and calcining to obtain a hydroxyl-rich porous carrier; S3, mixing the hydroxyl-rich porous carrier with an amino-containing silane coupling agent and performing an amination treatment to obtain an amination porous carrier; Then, the aminated porous carrier is reacted with a carboxyl-containing compound to obtain a carboxyl-grafted porous carrier; S4. Immerse the porous carrier grafted with carboxyl groups in a nickel salt solution and perform ultrasonic treatment, and then separate, dry and calcine to obtain a Ni-based reforming hydrogen production catalyst.
2. The method for preparing a reforming hydrogen production catalyst using waste vanadium-titanium denitration catalyst as raw material according to claim 1, characterized in that: In step S1, the concentration of the NaBH4 solution is 10-15%; The mixing ratio of the crushed vanadium titanium denitration catalyst and the NaBH4 solution is (3-5) g: (10-20) ml; The conditions for the heating and stirring reaction are: temperature 50-70°C, rotation speed 50-100 rpm, 0.5-1.5h; Drying conditions are: 85-120℃, 1-3h.
3. The method for preparing a reforming hydrogen production catalyst using waste vanadium-titanium denitration catalyst as raw material according to claim 1, characterized in that: In step S1, the molding agent is a 1-15wt% poly(ethylene) acid solution; The pore-forming agent is a 10-20wt% urea solution; The mass ratio of the obtained product to the forming agent and the pore-forming agent is (50-65):(3-10):(2-7); The calcination conditions are: 1000-1250°C, 1-2.5h.
4. The method for preparing a reforming hydrogen production catalyst using waste vanadium-titanium denitration catalyst as raw material according to claim 1, characterized in that: In step S2, the fluorine-containing ionic liquid is 1-butyl-3-methylimidazolium tetrafluoroborate; The mass ratio of the porous carrier to the fluorine-containing ionic liquid is (1-3):(5-8); The heating conditions are: 150-200°C, 15-25h; The calcination conditions are: 700-900°C, 1-2.5h.
5. The method for preparing a reforming hydrogen production catalyst using waste vanadium-titanium denitration catalyst as raw material according to claim 1, characterized in that: In step S3, the specific preparation method of the aminated porous carrier is: The hydroxyl-rich porous carrier, the amino-containing silane coupling agent, and anhydrous ethanol are mixed in a mass ratio of (2-4):1:(10-15), stirred at room temperature for 10-15 minutes, and then allowed to stand for 1-1.5 hours, filtered, and the filter residue is dried at 100-120°C for 1-2 hours; Wherein, the amino-containing silane coupling agent is (3-aminopropyl)triethoxysilane.
6. The method for preparing a reforming hydrogen production catalyst using waste vanadium-titanium denitration catalyst as raw material according to claim 1, characterized in that: In step S3, the specific preparation method of the carboxyl-grafted porous carrier is: The aminated porous carrier, the carboxyl-containing compound and DMF are mixed in a mass ratio of (2-5):(1-2):(10-20), stirred at room temperature for 15-25 minutes, allowed to stand for 1-2 hours, filtered, and the residue is dried at 110-130°C for 2-3 hours; Wherein, the carboxyl-containing compound is succinic anhydride.
7. The method for preparing a reforming hydrogen production catalyst using waste vanadium-titanium denitration catalyst as raw material according to claim 1, characterized in that: In step S4, the nickel salt is NiCl2·6H2O or Ni(NO3)2·6H2O or NiSO4·6H2O; The mass ratio of the carboxyl-grafted porous carrier to the nickel salt in the nickel salt solution is (8-12):(1-3).
8. The method for preparing a reforming hydrogen production catalyst using waste vanadium-titanium denitration catalyst as raw material according to claim 1, characterized in that: In step S4, the conditions for ultrasonic treatment are: 20-50 kHz, 0.5-1 h; Drying conditions are: 70-90°C, 1-1.5h; The calcination conditions are: 1100-1250°C, 0.5-2h.
9. A reforming hydrogen production catalyst, characterized in that: The method is prepared by any one of claims 1 to 8.
10. Use of the reforming hydrogen production catalyst prepared by the method according to any one of claims 1 to 8 or the reforming hydrogen production catalyst according to claim 9 in hydrogen production by steam reforming of methane.
Citation Information
Patent Citations
Preparation method and utilization method of catalyst originated from waste
CN107983362A
Reforming hydrogen production catalyst with waste vanadium-titanium denitration catalyst as raw material and preparation method of reforming hydrogen production catalyst
CN110302795A
Method for comprehensively recycling waste catalyst
CN114635032A
Reforming hydrogen production catalyst using waste vanadium-titanium denitration catalyst as raw material and preparation method therefor
WO2021012737A1
Cited By
Catalyst for preparing butanedioic anhydride through maleic anhydride hydrogenation and preparation method thereof
CN120306001A