Fluidized bed type airflow crushing device

Through the combined pickling method of fluidized bed airflow crushing and cold plasma gun, the problem of difficult removal of non-metallic impurities in metal silicon is solved, and low-temperature and efficient purification is achieved, energy consumption is reduced and the purity of silicon powder is improved. It is suitable for solar cells Production of materials.

CN118950197AInactive Publication Date: 2024-11-15ANYANG INST OF TECH
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202411217118.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-07
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing metal silicon impurity removal methods have problems such as high temperature, large energy consumption and unsatisfactory purification effects, especially it is difficult to effectively reduce the content of non-metallic element impurities such as B in silicon.

Method used

The fluidized bed airflow crushing device is used to combine a cold plasma gun and pickling method to crush the silicon material through high-pressure Ar gas and remove non-metal impurities by using cold plasma. Then, pickling liquid containing H2O2 and HF is used to pickling and remove impurities. Finally, the purification of high-purity silicon is achieved through directional solidification.

Benefits of technology

It realizes efficient removal of non-metallic impurities in metal silicon at low temperatures, reduces energy consumption, improves production efficiency, and the purity of silicon powder reaches the standard of solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950197A_ABST
    Figure CN118950197A_ABST
Patent Text Reader

Abstract

The fluidized bed type airflow crushing device comprises an isolation hood, and high-pressure silicon powder nozzles are symmetrically arranged on the lower portion of the side wall of the isolation hood; a high-pressure Ar gas inlet pipe is arranged at the bottom of the isolation hood; a cold plasma gun is arranged at the upper part of the isolation hood and is used for generating high-activity cold plasma substances; a silicon powder particle grading system is arranged at the upper part of the side wall of the isolation hood, and a silicon powder isolation film is arranged at the head part of the silicon powder particle grading system and is used for filtering large-particle silicon powder, so that the large-particle silicon powder returns to the isolation hood again, and small-particle silicon powder meeting requirements reaches a tail treatment system of the silicon powder particle grading system along with airflow; the tail treatment system is provided with an induced draft fan, a discharging barrel and a tail gas pipe, and the crushed and boron-removed silicon powder is discharged from the discharging barrel. According to the device, the silicon material crushing process and the boron removal process are completed in one step, the silicon material does not need to be melted at high temperature, the energy consumption is low, and the impurity removal effect is good.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of an invention patent application with an application date of March 7, 2023, application number 202310210768.0, and name “A method for removing metallic silicon impurities at low temperature”. Technical Field

[0002] The invention relates to a method for removing metallic silicon impurities at low temperature, belonging to the technical field of silicon material purification. The purified silicon powder can be used as a raw material for preparing solar cells. Background Art

[0003] Generally, metallic silicon (industrial silicon) is made by carbon reduction of quartz sand at high temperature (1800℃), with a purity of 99% (2N), and the content of boron (B) is between 30-50ppmw. Impurity elements in metallic silicon powder are divided into two categories: one is metallic element impurities, such as Fe, Al, Ca, Ti, etc., which are mainly located at the boundaries, defects and grain boundaries of crystalline silicon, and can be easily removed by acid pickling. The other is non-metallic element impurities, such as B, P (phosphorus), etc., which are located in the crystalline silicon crystal. Their segregation coefficient is relatively high, close to 1, and they cannot be removed by acid pickling and directional solidification. They are the two most difficult impurity elements to remove in metallic silicon. Element B is the culprit of the photoinduced degradation phenomenon of crystalline silicon solar cells. If its concentration is not reduced to below 0.3 ppmw, it will seriously affect the photoelectric conversion efficiency of solar cells.

[0004] There are four main methods for removing B from metallic silicon in the industry: complexation, slag making, blowing and plasma. Patent CN108328619A discloses "a method for removing boron from industrial silicon by hydrometallurgy". First, metallic silicon is made into porous silicon, and then the porous silicon is acid-washed and complexed. The boron removal rate can reach 93.3%, and the B content can be reduced from 13.2ppmw to 3ppmw, but it still cannot be used as solar silicon material. Patent ZL201010281559.8 discloses "a method for removing boron impurities from industrial silicon". Metallic silicon powder is added to a slag-making agent composed of SiO2 and alkali metal oxides, melted at high temperature, and element B is oxidized to boride (such as B2O) and overflows with the protective gas Ar gas. This method requires high temperature and high energy consumption, low production efficiency, and a large amount of slag-making agent. It cannot be applied to industrial production at present.

[0005] Patent CN102452651A discloses a process for removing boron impurities from silicon using wet argon plasma. The plasma gun input gas is argon, water vapor and oxygen, with a volume ratio of 30:1:1.5; the vacuum degree is 10 2The metal silicon in the crucible is melted in a resistance heat melting furnace of 1450-1550°C for 2-5 hours. This method needs to melt the silicon material at high temperature, which consumes a lot of energy and can only vaporize the element B on the surface of the silicon melt in the crucible. The concentration of element B in the silicon melt inside the crucible is difficult to reduce to the standard of solar silicon. Summary of the invention

[0006] In view of the problems existing in the prior art, the present invention provides a method for removing impurities from metallic silicon at low temperature, aiming to solve the problems of the existing metallic silicon impurity removal methods having high temperature, high energy consumption and less than ideal purification effect.

[0007] The technical solution of the present invention is as follows: A method for removing metallic silicon impurities at low temperature comprises the following steps: S1. Silicon material crushing and impurity removal: In a fluidized bed airflow crushing device, high-pressure Ar gas is used as a carrier to collide and crush silicon materials with a particle size of less than 1 mm to obtain silicon powder with a certain mesh size; a cold plasma gun is also installed on the fluidized bed airflow crushing device, and the cold plasma generated by the cold plasma gun removes non-metallic impurities from the crushed silicon powder; S2. Pickling and impurity removal: Use a pickling solution containing H2O2 and HF to pickle and impurity remove the silicon powder; S3, directional solidification and impurity removal, to obtain high-purity silicon with impurity content that meets the requirements of solar silicon.

[0008] Furthermore, the working material of the cold plasma gun is a mixture of Ar, H2, and H2O2.

[0009] Furthermore, an ICP analysis probe is installed on the fluidized bed airflow pulverizing device, and the ICP analysis probe is used to monitor the concentration of the generated gaseous boride.

[0010] Furthermore, before the pickling and impurity removal in step S2, the silicon powder is first heated at 300-400°C in air for a certain period of time.

[0011] Furthermore, the pickling solution in step S2 also contains a certain concentration of AgNO3 and propylene glycol.

[0012] Beneficial effects: The present invention first utilizes high-pressure Ar gas to carry silicon materials for collision to achieve the crushing of silicon materials, and simultaneously utilizes the high-activity cold plasma generated by a specific working substance containing hydrogen peroxide to treat the crushed silicon powder, thereby achieving the efficient removal of non-metallic impurities; then the silicon powder is pickled, and the pickling solution containing H2O2 and HF contains a certain concentration of AgNO3, which can corrode the silicon powder into porous silicon, which helps to efficiently remove most of the metal impurities and non-metallic impurities in the silicon powder; finally, after directional solidification, high-purity silicon with an impurity content that meets the requirements of solar-grade silicon is obtained. Compared with the prior art, the method for removing non-metallic impurities from metallic silicon described in the present invention does not require melting the silicon material at high temperature, has low energy consumption, and has a good impurity removal effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 It is a schematic diagram of a fluidized bed air flow pulverizing device. DETAILED DESCRIPTION

[0014] The present invention is described in detail below with reference to the accompanying drawings.

[0015] A method for removing impurities from metallic silicon at low temperature, comprising the following steps: ① Using a fluidized bed type air flow pulverizing device to pulverize metallic silicon, while introducing cold plasma to remove the impurity B in the metallic silicon, so that the content of B is reduced to a certain concentration, and other impurity elements P and C are also removed accordingly; the device enables the silicon material pulverization process and the "boron removal" process to be completed in one step, and the two promote each other, significantly reducing energy consumption and achieving high production efficiency. ② Pickling metallic silicon powder. ③ Directionally solidifying metallic silicon powder. The purity of the processed silicon powder can reach solar grade polysilicon. The invention technology has the characteristics of simple process, low energy consumption and high production efficiency, and can be applied in large-scale production. The specific steps are as follows.

[0016] The first step is to crush and deboronize the metal silicon. The crushing and deboronization of the metal silicon are carried out as follows: Figure 1The fluidized bed air flow pulverizing device shown in the figure. The device comprises an isolation cover 1, and a high-pressure silicon powder nozzle 2 is symmetrically arranged at the lower part of the side wall of the isolation cover 1. The silicon material with a particle size less than 1 mm is sprayed into the isolation cover by high-pressure argon gas as a carrier, and the silicon material is pulverized by the collision of the high-pressure airflow; a high-pressure Ar gas inlet pipe 3 is arranged at the bottom of the isolation cover to make the silicon material in the isolation cover in a boiling state. A cold plasma gun 4 is arranged at the upper part of the isolation cover to generate highly active cold plasma materials. The cold plasma can react with non-metallic impurities such as B, P, C in the silicon material to generate impurity gaseous materials and be discharged with argon gas. An ICP analysis probe 5 and a silicon powder particle classification system 6 are arranged at the upper part of the side wall of the isolation cover. The ICP analysis probe 5 is used to monitor the concentration of impurity gaseous materials such as gaseous boride generated in the isolation cover. A silicon powder isolation film 61 is provided at the head of the silicon powder particle grading system 6 to filter large-particle silicon powder and return the large-particle silicon powder to the isolation cover. Small-particle silicon powder that meets the requirements reaches the tail processing system 62 of the silicon powder particle grading system along with the air flow. The tail processing system 62 is provided with an induced draft fan, a discharge barrel and an exhaust pipe. The crushed and deboronized silicon powder is discharged from the discharge barrel.

[0017] The principle and process of metal silicon crushing and deboronization are as follows: metal silicon powder collides and rubs against each other in the fluidized bed isolation cover, and is cracked into fine particles at the silicon powder grain boundaries and defects, and the impurities B and P inside the silicon particles are exposed on the surface of the silicon particles. The silicon powder particle classification system contains a silicon powder isolation film, and the pores of the isolation film can be freely adjusted. The silicon powder particle size is controlled by the silicon powder particle classification mechanism to make its particle size meet the design standards.

[0018] The carbon steel composite material with high hardness, wear resistance and pressure resistance, strong cutting performance, smooth inner wall and not easy to rust is used as the isolation cover material to prevent silicon powder from adhering to the inner wall of the isolation cover. The working substances of the cold plasma gun are Ar, H2, and H2O2. In the process of silicon powder reacting with the active particles of cold plasma, a 5-10 nm SiO2 film is produced on the surface, which can prevent the ultra-fine silicon powder from agglomerating and bonding, and make the silicon powder crushed evenly. By controlling the composition, pressure and flow of the plasma working substance in the cold plasma gun, the degree of modification of the surface of the silicon powder by the plasma can be accurately controlled.

[0019] The cold plasma gun uses radio frequency glow discharge technology between the inner and outer electrodes, with a frequency of 13.56MHz and an AC voltage of 380V to generate cold plasma at a temperature of 800-1000℃. The working gas pressure is 8-10 Torr and the plasma gun power is 25 kW. The plasma temperature is related to the plasma gun AC frequency, AC voltage, plasma gun power, and working gas pressure.

[0020] The removal rate of B in silicon powder is proportional to the content of H2O2, the working substance in the plasma gun, the deboronization time, and the silicon powder loss rate.

[0021] The content of H2 in the plasma gun working substance is related to the deboronization efficiency. SiO2+2H→SiO(g)↑+H2O(g), hydrogen atoms can corrode the SiO2 film on the silicon surface and reduce the stability of the SiO2 film. It is beneficial for B atoms to migrate from the inside of the silicon body to the surface of the silicon powder (SiO2 film), react with plasma active particles, and improve the removal rate of boron elements in silicon powder. B+0.75SiO2→BO 1.5 +0.75Si, which is one of the reasons why cold plasma gun working material H2O2 is used for deboronation by doping with hydrogen (H2).

[0022] An offset electric field is added between the plasma gun and the bottom of the isolation cover to accelerate the flow speed of plasma active particles and reduce the time for silicon powder to be de-doped. The offset electric field voltage is set to a DC voltage (e.g. 126V).

[0023] An ICP-OES analysis probe is installed in the isolation cover to test the concentration of gaseous boride in real time online to determine the deboronization effect of silicon powder. If the B content of silicon powder is lower than a certain concentration and meets certain standards, the reaction is terminated.

[0024] In the cold plasma gun, hydrogen peroxide is ionized: H2O2→HO2 - +H + +O² - ;H2O2→2·OH; 2H2O2→2H2O+O2; H2O2+·OH→HO2·+H2O; H2O2+HO2·→·OH+H2O+O2; 2·OH→H2O2;·O - +H2O→HO·+HO - .

[0025] The cold plasma gun produces O, H, OH, and O after the working material is ionized. + OH - ,H2,O2,H2O,HO·,HO2·,·O2 - etc. + OH - , O2 can weaken Si-B bond. These active particles (such as hydrogen, oxygen atoms, ions or free radicals) react with B and P to form gaseous boride, which is drawn away with the silicon powder particle classification system, and the induced draft fan discharges the reaction tail gas and silicon powder, thereby achieving the purpose of purifying metallic silicon powder.

[0026] The activation energy of the reaction between plasma free radicals and impurities is very low, so the reaction speed is very fast and the formation of gaseous borides, phosphides and carbides is completed instantly.

[0027] Specifically, in the metal silicon crushing and boron removal device, the Ar gas high-pressure silicon powder nozzle pressure is set to 0.2-0.3MPa. Four silicon powder nozzles are arranged around the lower part of the isolation cover wall in a straight line symmetrical arrangement. At the intersection of the silicon powder, the silicon powders are violently impacted, collided, and rubbed against each other and crushed. The plasma gun is located 4-6 cm above the intersection of the silicon powder. During the silicon powder crushing process, the impurities exposed on the surface of the silicon powder react with the plasma active particles to generate a gaseous impurity phase. The silicon powder and the gaseous impurity phase (boride, phosphide, etc.) move with the rising argon gas flow to the silicon powder crushing particle grading mechanism. The coarse particles fall back to the lower part of the crushing chamber along the isolation cover wall under the action of gravity and undergo secondary crushing; the silicon powder dust and the gaseous impurity phase are discharged by the induced draft fan.

[0028] High-pressure Ar gas (0.2-0.3 MPa) is input from the middle of the bottom of the isolation cover to form a fluidized environment inside the isolation cover to achieve a fluidized bed effect. The falling silicon powder is suspended in the crushing area and reaction area for secondary crushing and secondary reaction.

[0029] The plasma active particles react with the impurities on the surface of the silicon powder to produce volatile borides, phosphides and carbides: 4 / 3B+O2→2 / 3B2O3; 4 / 5P+O2→2 / 5P2O5; H2O2+2H + →2H2O+2h + ;h + (Hole) has strong oxidation ability and can oxidize impurities such as B, P and C into gaseous impurity phases, 2B(s)+2H2O(g)+h + →2HBO(g)+H2(g); 4B(s)+3O2(g)+h + →2B2O3(g); 4B(s)+2H2O(g)+O2(g)→4HBO(g); The volatility of HBO is 1.5 orders of magnitude higher than that of BO; The volatility of BO is 1 order of magnitude higher than that of BH2. xB(s)+0.5yH2O(g)→4B x H y (g)+0.25yO2; B(s)+O+3H→HBO(g)↑+H2(g); B(s)+H2O(g)+H→HBO(g)+H2. C+O→CO(g)↑; 3H+P→PH3(g)↑. The hydrogen atoms in the plasma can also react with B, P and C in silicon to form volatile hydrides, such as BH 3、 PH3, CH4, etc.

[0030] The temperature at the intersection of silicon powder is about 80 to 200°C higher than the plasma temperature, which is caused by the plasma active particles bombarding the silicon powder. The heat generated by silicon oxidation can maintain the temperature of the plasma reaction zone. It is an effective method to remove the B element from metallic silicon by plasma method. The metallic silicon crushing and deboronization device designed by the present invention aims to improve the efficiency of metallic silicon deboronization and reduce the cost of deboronization. The key to the technology of this scheme is that the impurities in the silicon powder can fully contact with the plasma active substances to react.

[0031] The second step is pickling and impurity removal: Use a pickling solution containing HF to pickle and remove impurities from the silicon powder. Since the silicon powder is relatively fine, the impurity metal elements (Fe, Al, Ca, Ti) are mainly concentrated on the surface of the silicon powder, and B and P are also exposed on the surface of the silicon powder. In order to improve the impurity removal efficiency, the silicon powder can be heated at 300-400 degrees in the air for a certain period of time before pickling and impurity removal. For example, it can be heated to 300°C in a programmable box-type resistance furnace, kept warm for 0.5 h, and then annealed to form a layer of SiO2 film on the surface of the silicon powder. The silicon surface is modified and passivated. During the 300-degree insulation process of the silicon powder, the impurity element B will diffuse into the SiO2 film because the SiO2 film has an adsorption effect on B, and the affinity of oxygen (electronegativity 3.44) in SiO2 for B is greater than the affinity of Si (electronegativity 1.90) for B, SiO2+2X / yB→Si+2 / yB x O y ↑. Then hydrofluoric acid (HF) is used to pickle the metal silicon powder. Metallic impurities and non-metallic impurities are dissolved in the HF pickling solution along with the SiO2 film, SiO2+HF→SiF4↑+H2O. After negative pressure filtration of the pickling solution, silicon powder with significantly reduced impurity concentration is obtained.

[0032] The above-mentioned HF-containing pickling solution may also contain a certain concentration of H2O2 and AgNO3. The micron-sized silicon powder is corroded into porous silicon using the principle of the galvanic cell, and then the metal impurities and non-metallic impurities B and P in the polysilicon are removed by pickling to reduce the impurity content in the polysilicon. Metal Ag ions are added to the pickling solution, and the silver ions undergo a redox reaction and settle on the surface of the silicon powder. Under the catalytic action of the metal Ag atoms, the silicon powder is corroded into porous silicon, further exposing the impurity atoms such as B and P inside the silicon particles, which are easily removed by reaction with the pickling solution. Finally, the silver is dissolved and removed.

[0033] The third step is to use the traditional directional solidification method to make the purity of the final silicon material reach the standard of solar silicon.

[0034] The above-mentioned steps of air flow pulverization, plasma impurity removal, pickling impurity removal, directional solidification, etc. can be used alone or in combination, and can be specifically selected according to needs.

[0035] Application Examples

[0036] Case 1. The silicon powder was crushed to 325 mesh using a fluidized bed air flow pulverizing device. The plasma gun impurity removal process was not turned on during the process. The silicon powder was heated to 300°C in a programmable box-type resistance furnace, kept warm for 0.5-0.6 h, and then annealed. Since the silicon powder particles are fine and the median particle size is only 44μm, the heating temperature should not be too high, otherwise the silicon powder loss rate will be too high. After pickling with 2 mol / L HF for 3 hours, the silicon powder changed from hydrophilic to hydrophobic and floated on the surface of the pickling liquid, indicating that the SiO2 film on the surface of the silicon powder has been completely dissolved. Recovering the floating silicon powder can make the pickling process continuous. The test results show that the silicon recovery rate is 92.6%, and the silicon powder pickling results are shown in Table 1.

[0037]

[0038] Case 2. Metal silicon powder raw material, particle size 700-120 μm, purity 2N, using crushing and boron removal device, plasma gun working material 50Vol.%Ar+46Vol.%H2O2+4Vol. %H2, after 15min, most of the B in Si can be removed, the B removal efficiency reaches 98%, and the silicon powder recovery rate is 92%. If the H2 content in the working material is too low, the SiO2 film formed on the silicon surface will prevent the boride from volatilizing and affect the B removal rate. The correct H2 / H2O2 ratio can effectively prevent excessive oxidation of the silicon powder surface. The Fe and Cr content in the silicon powder after plasma treatment is still high, which is due to the sputtering of the cold plasma gun discharge electrode material and the isolation cover material. Then it is pickled and directionally solidified. Before pickling, the silicon powder was rotationally heated to 400°C in air at 13 r / h for 6 min. The pickling solutions were HF, HCl and H2SO4, all with a concentration of 2 mol / L. After directional solidification, the middle part of the silicon ingot was taken and its impurity concentration was tested by ICP-Ms. The results are shown in Table 2, which meet the requirements of solar polysilicon.

[0039]

[0040] Case 3. In a closed container, pickled silicon powder with a particle size of 700 μm-120 μm was pickled. The pickling solution composition was: 1 mol / L H2O2, 0.5 mol / L AgNO3, 2 mol / L HF, 0.1 mol / L propylene glycol. The mixture was heated to 70°C and stirred at 300 r / min for 2 hours. In the pickling solution, the metal atoms on the surface of the silicon powder replaced the silver ions. + Capture electrons from impure metal atoms (such as Al, Fe) in silicon powder, Al+3Ag + →Al 3+ +3Ag↓, the generated Ag atoms are deposited on the surface of silicon particles. Under the catalytic action of Ag atoms, a primary cell reaction occurs, 3Si+4NO3 - +16H+ +18F - →3SiF6 2- +4NO↑+8H2O, the silicon surface is corroded to form porous silicon, and the impurities on the silicon surface are dissolved in the pickling solution along with the fluorosilicic acid. In addition, with the participation of HF, H2O2+2H + →2H2O+2h + ,h + (Hole) has strong oxidation ability and can capture electrons in the valence band of silicon. Si+0.5H2O2+4HF→SiF4↑+H2O+1.5H2↑, and the silicon surface is also corroded. B+H + +NO3 - +H2O→H3BO3+NO↑, H3BO3+C3H8O3→BC3H5O3+3H2O, propylene glycol complexes boric acid to increase the release rate of B; 3P+5H + +5NO3 - +2H2O→3H3PO4+5NO↑. The valence band potential of Si is E valence =0.67V, the reduction potential of H2O2 is E H2O2 / H2O =1.763V, in HF solution, the h of H2O2 + It is easily injected into the valence band of Si. There are two purposes for adding glycerol to the pickling solution: one is to increase the solubility of the impurity B element in the pickling solution; the other is that the pickling solution has a strong corrosive ability on silicon powder, and silicon powder has an adsorption effect on glycerol, forming a thin shielding layer on the surface of silicon powder, slowing down the corrosion of the pickling solution on silicon powder and improving the recovery rate of silicon powder. Then use H2O2+NH3·H2O (volume ratio = 1.5:1) to wash the pickled silicon for 2 h to dissolve the Ag atoms therein, Ag+H2O2→Ag2O+H2O, Ag2O+4NH3·H2O→2[Ag(NH3)2]OH+3H2O, and finally use deionized water to wash the pickled silicon for a second time. The purity of the pickled silicon reaches 99.999%, of which the content of B is reduced from 34.30 to 0.99 ppmw, and the content of P is reduced from 48.60 to 1.78 ppmw.

[0041] Case 4. Silicon carbide (SiC) with a Mohs hardness of 9.3 at the micron level can also be crushed to 325 mesh using plasma and fluidized bed air flow crushing devices. Argon high-pressure nozzle 0.6 MPa, feed rate 80-130kg / h. The working material of the plasma gun is 96Vol.%Ar+4Vol.%H2O2. After 15 minutes, more than 87% of the SiC is crushed by mutual impact and collision between particles, and only less than 13% of the particles are crushed by collision and friction between the particles and the inner wall of the isolation cover. The SiC surface is modified, the particles are crushed evenly, and no agglomeration occurs.

Claims

1. A fluidized bed air flow pulverizing device, characterized in that: It includes an isolation cover, and a high-pressure silicon powder nozzle is symmetrically arranged at the lower part of the side wall of the isolation cover; a high-pressure Ar gas inlet pipe is arranged at the bottom of the isolation cover; a cold plasma gun is arranged at the upper part of the isolation cover, and the cold plasma gun is used to generate high-activity cold plasma material; a silicon powder particle grading system is arranged at the upper part of the side wall of the isolation cover, and a silicon powder isolation film is arranged at the head of the silicon powder particle grading system to filter large-particle silicon powder so that the large-particle silicon powder returns to the isolation cover, and small-particle silicon powder that meets the requirements reaches the tail processing system of the silicon powder particle grading system with the air flow, and the tail processing system is provided with an induced draft fan, a discharge barrel and a tail gas pipe, and the silicon powder that has been crushed and deboronated is discharged from the discharge barrel.

2. The fluidized bed type air flow pulverizing device according to claim 1, characterized in that: The number of the high-pressure silicon powder nozzles is 4. The high-pressure silicon powder nozzle uses high-pressure argon gas as a carrier to spray silicon materials with a particle size of less than 1 mm into the isolation cover, and the silicon materials are crushed by the collision of high-pressure airflow at the intersection of the silicon powders. At the same time, high-pressure Ar gas is introduced into the air inlet pipe at the bottom to make the silicon materials in the isolation cover boil. The cold plasma gun is located 4-6 cm higher than the intersection of the silicon powders.

3. The fluidized bed type air flow pulverizing device according to claim 2, characterized in that: The pressure of the high-pressure argon gas is 0.2-0.3 MPa.

4. The fluidized bed type air flow pulverizing device according to claim 1, characterized in that: The working material of the cold plasma gun is a mixture of Ar, H2, and H2O2. The highly active cold plasma material produced by the cold plasma gun can react with non-metallic impurities such as B, P, and C in the silicon material to generate impurity gaseous materials that are discharged along with the argon gas.

5. The fluidized bed type air flow pulverizing device according to claim 4, characterized in that: The temperature of the cold plasma generated by the cold plasma gun is 800-1000°C.

6. The fluidized bed type air flow pulverizing device according to claim 1, characterized in that: An ICP analysis probe is also installed on the upper part of the side wall of the isolation cover, and the ICP analysis probe is used to monitor the concentration of the generated gaseous boride.

Citation Information

Cited By

  • Dry grinding apparatus using plasma

    KR102928461B1

  • Dry nano-grinding system universally applicable to various solid raw materials

    KR102928462B1

  • Control method of dry grinding apparatus using plasma

    KR102928864B1

  • Dry nano-grinding method with improved particle size uniformity

    KR102970471B1

  • A apparatus for precisely controlling the particle size of nanoparticles to achieve quantum confinement effects

    KR102980794B1