Aero-engine single-crystal blade casting shell and method for judging drying of aero-engine single-crystal blade casting shell

Through multi-layer structural shell and high-temperature treatment technology, the durability problem of aero engine single crystal blade cast shell in high temperature environment is solved, and stable casting above 1500℃ is achieved.

CN118950938APending Publication Date: 2024-11-15CHENGDU ENGINE GROUP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411040374.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The cast shell of the existing aircraft engine single crystal blade is difficult to last for a long time in high temperature environments, and it is prone to defects such as cracking, swelling and fire-running during casting.

Method used

Using a shaped shell structure consisting of a surface layer, a transition layer, an intermediate layer and a sealing layer, it is prepared using materials such as silicon sol and high-purity high-alumina mullite powder, and a multi-layer structure is formed through specific slurry mixing, sand hanging and drying steps. , and steam loss and pre-baking treatment are carried out at high temperature to ensure the high temperature resistance of the molded shell above 1500°C.

Benefits of technology

During the pouring process, the shell can slowly pull out in a high temperature environment of more than 1500℃, without defects such as rupture, expansion and fire running, which significantly improves the high temperature resistance of the shell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950938A_ABST
    Figure CN118950938A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of material forming investment precision casting, and particularly relates to an aero-engine single-crystal blade casting shell and a method for judging drying of the aero-engine single-crystal blade casting shell, and the aero-engine single-crystal blade casting shell comprises a surface layer, a transition layer, a middle layer and a sealing layer from inside to outside; the surface layer is prepared from the following raw materials: silica sol, electric smelting high-purity high-aluminum mullite powder with the granularity of 300-350 meshes and white corundum sand with the granularity of 60-80 meshes; the content ratio of the silica sol to the electric smelting high-purity high-aluminum mullite powder is (2: 1)-(4: 1); the preparation raw material of the transition layer comprises electric smelting high-purity high-aluminum mullite sand; the surface granularity of the transition layer is 32-40 meshes; according to the invention, the long-time high-temperature resistance of the shell under the environment of more than 1500 DEG C can be ensured in the manufacturing process of a smelting and pouring process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of material forming investment casting, and in particular relates to a casting shell of a single crystal blade of an aero-engine and a method for judging its drying. Background Art

[0002] In the field of aviation technology, the working environment of precision-cast blade parts of aircraft engines is harsh. High-temperature parts work at high temperatures for a long time, which places stringent requirements on the performance of the parts used. Blades produced using directional solidification casting technology can better adapt to high-temperature working environments and ensure the performance of blades.

[0003] Therefore, manufacturing single crystal casting blades is the key to improving the performance of aircraft engines and the key to the ability of blade body aviation investment casting process. To ensure the manufacturing environment of the smelting and pouring process for producing single crystal casting blades, the shell is slowly pulled at a speed of several millimeters per minute in a heated environment to form a temperature field of sequential solidification. Therefore, it is necessary to formulate a reasonable single crystal shell manufacturing process to ensure that the shell can withstand high temperatures for a long time in an environment exceeding 1500°C during the smelting and pouring process. Summary of the invention

[0004] In view of this, the present invention provides a casting shell of a single crystal blade of an aircraft engine and a method for judging its dryness. The shell includes a surface layer, a transition layer, an intermediate layer and a sealing layer from the inside to the outside, so as to ensure that the shell can withstand high temperatures exceeding 1500°C for a long time during the smelting and pouring process.

[0005] The technical solution adopted by the present invention is:

[0006] A casting shell for a single crystal blade of an aero-engine, the shell comprising a surface layer, a transition layer, an intermediate layer and a sealing layer from the inside to the outside;

[0007] The raw materials for preparing the surface layer include silica sol, fused high-purity high-aluminum mullite powder with a particle size of 300-350 meshes, and white corundum sand with a particle size of 60-80 meshes; the content ratio of the silica sol to the fused high-purity high-aluminum mullite powder is 2:1-4:1;

[0008] The raw material for preparing the transition layer includes fused high-purity high-aluminum mullite sand; the surface particle size of the transition layer is 32-40 mesh;

[0009] The raw materials for preparing the intermediate layer include silica sol and fused high-purity high-aluminum mullite powder with a particle size of 300-350 mesh; the content ratio of the silica sol to the fused high-purity high-aluminum mullite powder is 2:1-3:1;

[0010] Wherein: the number of the transition layers is greater than or equal to 2 layers

[0011] Furthermore, the method for preparing the slurry of the surface layer comprises the following steps:

[0012] S101: Mix quick-drying silica sol and fused high-purity high-aluminum mullite powder in a ratio of 2:1-4:1, stir until the viscosity is between 40s and 60s, and let stand for more than 12 hours;

[0013] S102: Stir again for more than 5 minutes until the viscosity is less than 30 seconds;

[0014] Furthermore, the method for preparing the slurry of the intermediate layer comprises the following steps:

[0015] Mix quick-drying silica sol and fused high-purity high-alumina mullite powder in a ratio of 2:1 to 3:1, and stir until the Jan's viscosity is below 10s.

[0016] Furthermore, the preparation method of the surface layer comprises the following steps:

[0017] S201: Immersing the wax mold assembly into the slurry of the surface layer;

[0018] S202: Control the material of the wax mold module after the material is soaked and hang white corundum sand, the sand hanging particle size is 60-80 mesh;

[0019] S203: Drying the surface layer after sanding.

[0020] Furthermore, the method for preparing the transition layer comprises the following steps:

[0021] S301: Immersing the wax mold module obtained in S203 into the slurry of the middle layer;

[0022] S302: Control the material of the wax mold module after the material is soaked and hang the fused high-purity high-aluminum mullite sand, the sand hanging particle size is 32-40 mesh;

[0023] S303: Drying the transition layer after sanding.

[0024] Furthermore, the method for preparing the intermediate layer comprises the following steps:

[0025] S401: Immersing the wax mold module obtained in S303 into the slurry of the middle layer;

[0026] S402: Control the material of the wax mold module after the material is soaked and hang the fused high-purity high-aluminum mullite sand, the sand hanging particle size is 20-35 mesh;

[0027] S403: Drying the middle layer of the current layer after sanding;

[0028] S404: Repeat the steps S401-S403 on the basis of the dried intermediate layer until all the intermediate layers are formed.

[0029] Furthermore, the preparation method of the sealing layer comprises the following steps:

[0030] S501: Immersing the wax mold module obtained in S403 into the slurry of the middle layer;

[0031] S502: Controlling the material of the wax mold module after the dip;

[0032] S503: Drying the sealed layer after material control.

[0033] Furthermore, after S503, the following steps are also included:

[0034] S601: performing steam lost wax treatment on the ceramic shell obtained in S503;

[0035] The lost wax process is completed based on a steam dewaxing kettle, the pressure of the dewaxing outer tank of the steam dewaxing kettle is not less than 0.4Mpa, and the dewaxing time is 5-20min.

[0036] Furthermore, after S601, the step further includes the following steps:

[0037] Pre-baking the lost wax shell;

[0038] The pre-baking process is completed in a baking furnace, and the specific process is: after the shell is placed in the baking furnace, the baking furnace is heated freely to 620-680°C, kept warm for 0.5-3h, and then heated to 800°C-900°C, kept warm for 1.5-3h.

[0039] Furthermore, assuming that the maximum thickness of the shell is h max , the thickness difference between the minimum thickness and the maximum thickness is Δh; then the Δh is not greater than h max 5-20% of.

[0040] The present invention also proposes a method for determining whether the casting shell of the above-mentioned single crystal blade of the aero-engine is dry:

[0041] Assuming that the weight of the wax mold module before S201 is w1, the weight of the wax mold module before S201 is w2, and the weight of the wax mold module after each drying process is w3, then:

[0042] αρ(w2-w1)=(w2-w3)

[0043] Where: α is the drying coefficient, ρ is the mass fraction of liquid phase in the slurry;

[0044] The α value of the surface layer is 0.95-0.998, the α value of the transition layer is 0.95-0.998, the α value of the middle layer is 0.98-0.999, and the α value of the sealing layer is 0.99-0.999.

[0045] Beneficial effects of the present invention:

[0046] The aero-engine single crystal blade casting mold shell of the present invention is placed in a high-temperature heater with upper and lower temperature zones exceeding 1500° C. during the pouring process. When the inner cavity of the mold shell is subjected to alloy liquid exceeding 1500° C., it can be slowly pulled out of the heater for 1 hour to 2 hours without defects such as mold cracking, bulging, and sparking occurring during the pouring and solidification processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0048] Figure 1 It is a schematic structural diagram of a casting shell of a single crystal blade of an aero-engine in a specific embodiment of the present invention;

[0049] Figure 2 A schematic diagram of the thickness distribution of a casting shell of a single crystal blade of an aircraft engine in a specific embodiment of the present invention;

[0050] Among them: 1. Surface layer; 2. Transition layer; 3. Middle layer; 4. Closing layer. DETAILED DESCRIPTION

[0051] The embodiments of the present disclosure are described in detail below with reference to the accompanying drawings.

[0052] The following describes the embodiments of the present disclosure through specific examples, and those skilled in the art can easily understand other advantages and effects of the present disclosure from the contents disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of the present disclosure, rather than all of the embodiments. The present disclosure can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present disclosure. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present disclosure.

[0053] It should be noted that various aspects of the embodiments within the scope of the appended claims are described below. It should be apparent that the aspects described herein may be embodied in a wide variety of forms, and any specific structure and / or function described herein is merely illustrative. Based on the present disclosure, it should be understood by those skilled in the art that an aspect described herein may be implemented independently of any other aspect, and two or more of these aspects may be combined in various ways. For example, any number of aspects described herein may be used to implement a device and / or practice a method. In addition, other structures and / or functionalities other than one or more of the aspects described herein may be used to implement this device and / or practice this method.

[0054] It should also be noted that the illustrations provided in the following embodiments are only schematic illustrations of the basic concept of the present disclosure. The drawings only show components related to the present disclosure rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0055] Additionally, in the following description, specific details are provided to facilitate a thorough understanding of the examples. However, it will be understood by those skilled in the art that the aspects described may be practiced without these specific details.

[0056] In one embodiment of the present invention, a single crystal blade casting shell for an aero-engine is provided, such as Figure 1 As shown, the shell includes a surface layer 1, a transition layer 2, an intermediate layer 3 and a sealing layer 4 from the inside to the outside;

[0057] The raw materials for preparing the surface layer 1 include silica sol, fused high-purity high-aluminum mullite powder with a particle size of 300-350 meshes, and white corundum sand with a particle size of 60-80 meshes; the content ratio of silica sol to fused high-purity high-aluminum mullite powder is 2:1-4:1;

[0058] The raw materials for preparing the transition layer 2 include fused high-purity high-aluminum mullite sand; the surface particle size of the transition layer 2 is 32-40 mesh;

[0059] The raw materials for preparing the intermediate layer 3 include silica sol and fused high-purity high-aluminum mullite powder with a particle size of 300-350 mesh; the content ratio of silica sol to fused high-purity high-aluminum mullite powder is 2:1-3:1;

[0060] Among them: the number of transition layers 2 is greater than or equal to 2 layers (whether there is sand hanging and drying between each layer)

[0061] In this embodiment, the slurry preparation method of the surface layer 1 includes the following steps:

[0062] S101: Mix quick-drying silica sol and fused high-purity high-aluminum mullite powder in a ratio of 2:1-4:1, stir until the viscosity is between 40s and 60s, and let stand for more than 12 hours;

[0063] S102: Stir again for more than 5 minutes until the viscosity is less than 30 seconds;

[0064] In this embodiment, the method for preparing the slurry of the intermediate layer 3 comprises the following steps:

[0065] Mix quick-drying silica sol and fused high-purity high-alumina mullite powder in a ratio of 2:1 to 3:1, and stir until the Jan's viscosity is below 10s.

[0066] In this embodiment, the preparation method of the surface layer 1 includes the following steps:

[0067] S201: Immerse the wax mold assembly into the slurry of the surface layer 1;

[0068] S202: Control the material of the wax mold module after the material is soaked and hang white corundum sand, the sand hanging particle size is 60-80 mesh;

[0069] S203: Drying the surface layer 1 after sanding.

[0070] In this embodiment, the preparation method of the transition layer 2 includes the following steps:

[0071] S301: Immerse the wax mold module obtained in S203 into the slurry of the middle layer 3;

[0072] S302: Control the material of the wax mold module after the material is soaked and hang the fused high-purity high-aluminum mullite sand, the sand hanging particle size is 32-40 mesh;

[0073] S303: Drying the transition layer 2 after sanding.

[0074] In this embodiment, the preparation method of the intermediate layer 3 includes the following steps:

[0075] S401: Immerse the wax mold module obtained in S303 into the slurry of the middle layer 3;

[0076] S402: Control the material of the wax mold module after the material is soaked and hang the fused high-purity high-aluminum mullite sand, the sand hanging particle size is 20-35 mesh;

[0077] S403: Drying the middle layer of the current layer after sanding;

[0078] S404: Repeat the steps S401-S403 on the basis of the dried intermediate layer until all the intermediate layers 3 are formed.

[0079] In this embodiment, the preparation method of the sealing layer 4 includes the following steps:

[0080] S501: Immerse the wax mold module obtained in S403 into the slurry of the middle layer 3;

[0081] S502: Controlling the material of the wax mold module after the dip;

[0082] S503: Drying the sealed layer 4 after material control.

[0083] In this embodiment, the following steps are further included after S503:

[0084] S601: performing steam lost wax treatment on the ceramic shell obtained in S503;

[0085] Among them, the lost wax process is completed based on a steam dewaxing kettle, and the dewaxing outer tank pressure of the steam dewaxing kettle is not less than 0.4Mpa; the dewaxing time is 5-20min.

[0086] In this embodiment, the following steps are further included after S601:

[0087] Pre-baking the lost wax shell;

[0088] Among them, the pre-baking process is completed based on the baking furnace. The specific process is: after the shell is placed in the baking furnace, the baking furnace is heated freely to 620-680℃, kept warm for 0.5-3h, and then heated to 800℃-900℃, kept warm for 1.5-3h.

[0089] In some embodiments, Figure 2 As shown, assuming that the maximum thickness of the shell is h max , the thickness difference between the minimum thickness and the maximum thickness is Δh; then the Δh is not greater than h max 5-20% of Δh vs h max It can be measured by X-ray, ultrasonic thickness gauge, and anatomical measurement.

[0090] The overall process of manufacturing the shell for the single crystal blade of the aircraft engine in this embodiment is as follows:

[0091] 1. Single crystal ceramic shell material:

[0092] High purity silica sol; fused corundum sand 60-80# (mesh); quick drying silica sol; fused high purity high aluminum mullite sand 20-35# and 30-40#; fused high purity high aluminum mullite powder 300-350 mesh.

[0093] 2 Slurry preparation

[0094] a. Preparation of surface layer 1 slurry: Use a fast mixer to mix silica sol and fused high-purity high-aluminum mullite powder in a ratio of 2:1-4:1, and stir until the viscosity is between 40s and 60s. According to the viscosity, you can add fused high-purity high-aluminum mullite powder or silica sol to fine-tune the viscosity to ensure that the viscosity meets the requirements. After standing for ≥12h to mature the slurry, stir again for ≥5min, and use it after the viscosity is re-measured and is less than 30s.

[0095] b. Preparation of the slurry for the intermediate layer 3: Use a fast mixer to mix quick-drying silica sol and fused high-purity high-aluminum mullite powder in a ratio of about 2:1 to 3:1, and stir until the viscosity is below 10s. Powder or silica sol can be added to fine-tune the viscosity according to the viscosity to ensure that the viscosity meets the viscosity requirements before use.

[0096] Note: If there are too many bubbles during the stirring process, defoaming agent can be added as appropriate.

[0097] 2 Shell making process:

[0098] a. Surface layer 1 Shell making process

[0099] Immerse the wax model module into the surface layer 1 slurry, take out the controlled material and then sand it, using white corundum sand with a particle size of 60-80#.

[0100] Drying time: ≥8h.

[0101] b. Second layer shell making process (transition layer 2)

[0102] Immerse the wax mold module into the multi-layer slurry, take out the controlled material and then hang sand, hang electric fused high-purity high-aluminum mullite sand with a particle size of 36 mesh.

[0103] Drying time: ≥4h

[0104] c. Shell making process of layer 3-n (intermediate layer 3)

[0105] Immerse the wax mold module in multiple layers of slurry, take out the controlled material and then hang sand, hang electric fused high-purity high-aluminum mullite sand with a particle size of 20-35#.

[0106] Drying time: ≥2h

[0107] d. Sealing layer 4

[0108] Immerse the wax mold assembly into the last multi-layer slurry (middle layer 3 slurry), take out the controlled material, and dry it.

[0109] Drying time: ≥2h

[0110] Note 1: n≥4, determined comprehensively based on the high temperature resistance of the mold shell, the size of the module and the quality of single crystal growth.

[0111] Note 2: Viscosity tests are all carried out using a James cup.

[0112] 3. Steam lost wax ceramic shell

[0113] The shell is placed in a steam dewaxing kettle, and the pressure of the dewaxing outer tank is not less than 0.4Mpa; the dewaxing time is 5-20min.

[0114] 4. Pre-baking of ceramic shell

[0115] The shell is placed in a baking furnace, and the temperature is freely raised to 620-680°C, and kept at this temperature for 0.5-3h, and then raised to 800°C-900°C, and kept at this temperature for 1.5-3h.

[0116] 5 After cooling down, clean the inner cavity, seal the pouring cup and bottom for later use.

[0117] In one embodiment, the present invention further proposes a method for judging the drying of the casting shell of the single crystal blade of the aircraft engine in the above embodiment: assuming that the weight of the wax mold module before S201 is w1, the weight of the wax mold module before S201 is w2, and the weight of the wax mold module after each drying process is w3, then:

[0118] αρ(w2-w1)=(w2-w3)

[0119] Where: α is the drying coefficient, ρ is the mass fraction of liquid phase in the slurry;

[0120] The α value of the surface layer is 0.95-0.998, the α value of the transition layer is 0.95-0.998, the α value of the middle layer is 0.98-0.999, and the α value of the sealing layer is 0.99-0.999.

[0121] The above is only a specific implementation of the present disclosure, but the protection scope of the present disclosure is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present disclosure should be included in the protection scope of the present disclosure. Therefore, the protection scope of the present disclosure should be based on the protection scope of the claims.

Claims

1. A single crystal blade casting shell for an aero-engine, characterized in that: The shell comprises a surface layer, a transition layer, an intermediate layer and a sealing layer from the inside to the outside; The raw materials for preparing the surface layer include silica sol, fused high-purity high-aluminum mullite powder with a particle size of 300-350 meshes, and white corundum sand with a particle size of 60-80 meshes; the content ratio of the silica sol to the fused high-purity high-aluminum mullite powder is 2:1-4:1; The raw material for preparing the transition layer includes fused high-purity high-aluminum mullite sand; the surface particle size of the transition layer is 32-40 mesh; The raw materials for preparing the intermediate layer include silica sol and fused high-purity high-aluminum mullite powder with a particle size of 300-350 mesh; the content ratio of the silica sol to the fused high-purity high-aluminum mullite powder is 2:1-3:1; Wherein: the number of the transition layers is greater than or equal to 2 layers.

2. The single crystal blade casting shell of an aircraft engine according to claim 1, characterized in that: The method for preparing the slurry of the surface layer comprises the following steps: S101: Mix quick-drying silica sol and fused high-purity high-aluminum mullite powder in a ratio of 2:1-4:1, stir until the viscosity is between 40s and 60s, and let stand for more than 12 hours; S102: Stir again for more than 5 minutes until the viscosity is less than 30 seconds.

3. The single crystal blade casting shell of an aircraft engine according to claim 2, characterized in that: The method for preparing the slurry of the intermediate layer comprises the following steps: Mix quick-drying silica sol and fused high-purity high-alumina mullite powder in a ratio of 2:1 to 3:1, and stir until the Jan's viscosity is below 10s.

4. The single crystal blade casting shell of an aircraft engine according to claim 3, characterized in that: The preparation method of the surface layer comprises the following steps: S201: Immersing the wax mold assembly into the slurry of the surface layer; S202: Control the material of the wax mold module after the material is soaked and hang white corundum sand, the sand hanging particle size is 60-80 mesh; S203: Drying the surface layer after sanding.

5. The single crystal blade casting shell of an aircraft engine according to claim 4, characterized in that: The preparation method of the transition layer comprises the following steps: S301: Immersing the wax mold module obtained in S203 into the slurry of the middle layer; S302: Control the material of the wax mold module after the material is soaked and hang the fused high-purity high-aluminum mullite sand, the sand hanging particle size is 32-40 mesh; S303: Drying the transition layer after sanding.

6. The single crystal blade casting shell of an aircraft engine according to claim 5, characterized in that: The preparation method of the intermediate layer comprises the following steps: S401: Immersing the wax mold module obtained in S303 into the slurry of the middle layer; S402: Control the material of the wax mold module after the material is soaked and hang the fused high-purity high-aluminum mullite sand, the sand hanging particle size is 20-35 mesh; S403: Drying the middle layer of the current layer after sanding; S404: Repeat the steps S401-S403 on the basis of the dried intermediate layer until all the intermediate layers are formed.

7. The aero-engine single crystal blade casting shell according to claim 6, characterized in that: The preparation method of the sealing layer comprises the following steps: S501: Immersing the wax mold module obtained in S403 into the slurry of the middle layer; S502: Controlling the material of the wax mold module after the dip; S503: Drying the sealed layer after material control.

8. The single crystal blade casting shell of an aircraft engine according to claim 7, characterized in that: After S503, the following steps are also included: S601: performing steam lost wax treatment on the ceramic shell obtained in S503; The lost wax process is completed based on a steam dewaxing kettle, the dewaxing outer tank pressure of the steam dewaxing kettle is not less than 0.4Mpa; the dewaxing time is 5-20min; The step S601 further includes the following steps: Pre-baking the lost wax shell; The pre-baking process is completed in a baking furnace, and the specific process is: after the shell is placed in the baking furnace, the baking furnace is heated freely to 620-680°C, kept warm for 0.5-3h, and then heated to 800°C-900°C, kept warm for 1.5-3h.

9. The single crystal blade casting shell of an aircraft engine according to claim 7, characterized in that: Assume that the maximum thickness of the shell is h max , the thickness difference between the minimum thickness and the maximum thickness is Δh; then the Δh is not greater than h max 5-20% of.

10. The method for judging the dryness of the casting shell of the single crystal blade of the aircraft engine according to any one of claims 1 to 9, characterized in that: Assuming that the weight of the wax mold module before S201 is w1, the weight of the wax mold module before S201 is w2, and the weight of the wax mold module after each drying process is w3, then: αρ(w2-w1)=(w2-w3) Where: α is the drying coefficient, ρ is the mass fraction of liquid phase in the slurry; The α value of the surface layer is 0.95-0.998, the α value of the transition layer is 0.95-0.998, the α value of the middle layer is 0.98-0.999, and the α value of the sealing layer is 0.99-0.999.