Method for preparing carbon fiber cloth reinforced aluminum-based composite board by adopting semi-solid cast rolling method

The continuous infiltration of nickel-plated carbon fiber braided fabrics through semi-solid casting and rolling method solves the problem of insufficient matrix penetration capacity in carbon fiber reinforced aluminum matrix composite materials, and achieves high-quality and short-process composite effects, which are suitable for large-scale production.

CN118950960AActive Publication Date: 2024-11-15NORTHEASTERN UNIV CHINA
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411455195.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-11-15
Estimated Expiration
2044-10-18

AI Technical Summary

Technical Problem

The casting process of existing carbon fiber reinforced aluminum-based composite materials cannot take into account the composite quality and production efficiency. Especially when the carbon fiber cloth reinforced aluminum-based composite sheet is prepared, the matrix permeability and fiber protection capacity are insufficient, resulting in difficult to guarantee the composite quality and long production cycle.

Method used

The nickel-plated carbon fiber braided fabric is continuously immersed by the semi-solid casting and rolling method. The aluminum alloy semi-solid slurry and the carbon fiber braided fabric are applied through the rolling roll to firmly combine the aluminum alloy semi-solid slurry with the carbon fiber braided fabric, achieving high-quality and short-process compounding effect.

Benefits of technology

The efficient penetration of carbon fiber and aluminum alloy is achieved in the non-confined space, ensuring the structural integrity and performance of composite sheets, simplifying the process flow, reducing costs, and suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950960A_ABST
    Figure CN118950960A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a carbon fiber cloth reinforced aluminum-based composite board by adopting a semi-solid cast rolling method, and belongs to the field of metal material casting. The invention provides a high-quality and short-process preparation method for preparing a carbon fiber woven cloth reinforced aluminum-based composite board by adopting a semi-solid cast-rolling method, and the cast-rolling method is utilized to continuously provide pressure to drive aluminum alloy semi-solid slurry to continuously infiltrate nickel-plated carbon fiber woven cloth and form firm combination with the nickel-plated carbon fiber woven cloth. The barrier of insufficient wettability between a fiber reinforcement body and a matrix in traditional composite board manufacturing is broken through, and a high-quality composite effect is obtained based on a short-process technology in a non-closed space.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metal material casting, and in particular relates to a method for preparing a carbon fiber cloth reinforced aluminum-based composite plate by adopting a semi-solid casting and rolling method. Background Art

[0002] Carbon fiber reinforced aluminum-based composite materials are composite materials with aluminum or aluminum alloy as the matrix and carbon fiber as the reinforcement. They have the advantages of light weight, high strength, good electrical and thermal conductivity, no moisture absorption, and no aging. They have become ideal materials in the context of energy conservation, emission reduction, low carbon and environmental protection, and have great application potential in modern industry, especially in the field of high-tech. Among them, carbon fiber cloth refers to a two-dimensional woven cloth with different fiber arrangement directions obtained by weaving based on continuous unidirectional fibers. This form of reinforcement can effectively avoid the occurrence of a large number of fiber fractures, and has the ability of multi-directional synchronous strengthening. It can also carry out targeted design of fiber arrangement according to the actual service environment, ensuring the lightweight effect of the material to a greater extent. It is an ideal form of fiber implantation.

[0003] In the traditional casting composite method of carbon fiber reinforced aluminum-based composite materials, due to the large difference in density between carbon and aluminum, it is difficult to evenly distribute carbon fibers, and the wetting ability of aluminum melt on carbon fibers is extremely poor. The infiltration process between the two can often only be completed by external driving force. At present, the commonly used infiltration driving mechanisms can be divided into: 1. The forced pressing effect of the matrix on the carbon fibers in a closed mold; 2. The impact effect of the matrix movement on the carbon fibers in a non-closed environment. The former has strong infiltration ability and high interface controllability, but the production cycle is long and the product size is limited; the latter has a short production process, but poor infiltration ability and difficult to guarantee composite quality. In addition, when preparing carbon fiber cloth reinforced aluminum-based composite sheets, due to its own structural limitations, the preparation process is often required to have higher matrix penetration ability and stronger fiber protection ability.

[0004] Based on the above situation, the development of high-quality, short-process preparation technology for carbon fiber woven cloth reinforced aluminum-based composite panels has become an urgent problem to be solved in order to promote the widespread practical application of this ideal lightweight material. Summary of the invention

[0005] In view of the problem that existing carbon fiber reinforced aluminum-based composite sheet preparation processes cannot take into account both composite quality and production efficiency, the present invention proposes a high-quality, short-process preparation method for preparing carbon fiber woven cloth reinforced aluminum-based composite sheet using a semi-solid casting and rolling method. The casting and rolling method is used to continuously provide pressure to drive the aluminum alloy semi-solid slurry to continuously infiltrate the nickel-plated carbon fiber woven cloth and form a strong bond with it. The purpose is to break the barrier of insufficient wettability between the fiber reinforcement and the matrix in the manufacture of traditional composite sheets, and to obtain a high-quality composite effect based on a short-process technology in a non-confined space.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] A method for preparing a carbon fiber cloth reinforced aluminum-based composite plate by a semi-solid casting and rolling method, wherein the carbon fiber cloth is a carbon fiber woven cloth, and the method comprises the following steps: Step 1: Surface metallization of carbon fiber woven cloth: Step 1.1. Surface glue removal: In an atmospheric environment, burn the carbon fiber woven fabric at 450℃-500℃ for 30min-45min; Step 1.2. Surface degreasing: Use a mixture containing 55g / L-65g / L NaOH, 15g / L-25g / L Na 2 CO 3 and 35g / L-45g / L Na 3 PO 4 The 70℃-80℃ ternary alkaline aqueous solution is used as a degreasing agent, and the carbon fiber woven fabric after degumming is degreased for 20min-40min under the action of ultrasonic vibration, and then the degreased carbon fiber woven fabric is cleaned until there is no degreasing agent residue on the surface; Step 1.3. Surface etching: using 50g / L-70g / L H 2 SO 4 、200g / L-300g / L(NH 4 ) 2 S 2 O 8 A 40-60°C aqueous solution is used as an etchant, and the carbon fiber woven fabric after surface degreasing is etched for 15-20 minutes under the action of ultrasonic vibration, and then the etched carbon fiber woven fabric is cleaned until there is no etchant residue on the surface; Step 1.4. Surface sensitization: Place the etched carbon fiber weave in a 30℃-40℃ solution containing 10g / L-20g / L SnCl 2 And 30mL / L-40mL / L HCl sensitizing solution for 25min-30min ultrasonic vibration treatment to form a uniform layer of Sn on its surface 2 (OH) 3 Cl adsorption layer, and then clean the surface-sensitized carbon fiber woven cloth until there is no sensitizing liquid residue on the surface; Step 1.5. Surface activation: using 0.5g / L-1g / L PdCl 2 , using 10mL / L-20mL / L HCl aqueous solution as an activation solution, performing an activation treatment on the surface-sensitized carbon fiber woven fabric at a temperature of 50°C-70°C for 25min-30min, and then washing the activated carbon fiber woven fabric until no activation solution remains on the surface; Step 1.6. Surface deposition: 15g / L-20g / L NiSO 4 6H 2 O as main salt, 15g / L-20g / LNaH 2 PO 2 ·H 2 O as a reducing agent, 15mL / L-20mL / L lactic acid as a stabilizer, 1g / L-3g / L sodium dodecylbenzene sulfonate as a dispersant, and deposition is performed at pH = 3.5-4.5 and 70°C-80°C for 30min-120min to obtain a surface nickel-plated carbon fiber woven fabric; Step 2: Preparation of semi-solid aluminum alloy matrix: Step 2.1. Material selection: Select aluminum alloy raw materials with corresponding components according to needs; Step 2.2. Melting: melt the aluminum alloy raw material in an induction furnace, stir it evenly with a graphite stirring paddle after it is completely melted, and obtain the corresponding aluminum alloy liquid; wherein the melting temperature is 40°C-60°C higher than the liquidus line of the corresponding aluminum alloy; Step 2.3. Preparation of aluminum alloy semi-solid slurry: The aluminum alloy liquid obtained in step 2.2 is subjected to refining and degassing treatment and then cooled. When the temperature of the aluminum alloy liquid is cooled to 10°C higher than the melting point, mechanical stirring is applied and the temperature is continued to be cooled. After obtaining an aluminum alloy semi-solid slurry with a solid phase ratio of 25%-40%, stirring is stopped and the slurry is kept warm for casting and rolling. The stirring speed of the mechanical stirring is 1500r / min, and the stirring time depends on the specific cooling rate. Step 3: Semi-solid casting and rolling of nickel-plated carbon fiber woven cloth and aluminum alloy matrix: Step 3.1. Preheat the surface nickel-plated carbon fiber woven fabric to 350°C-400°C, introduce it into the front insulation chamber of the casting and rolling mill, pass it through the center of the roller, and put it in a tensioned state; Step 3.2. Use a flat-injection twin-roll casting and rolling equipment; introduce the aluminum alloy semi-solid slurry into the insulation chamber in front of the casting and rolling machine, and start casting and rolling after the temperature is measured by the temperature measuring system; after the aluminum alloy semi-solid slurry passes through the guide groove and the casting nozzle, it enters between the rollers from the insulation chamber, so that the upper and lower layers of the nickel-plated carbon fiber woven cloth are both aluminum alloy semi-solid slurry, and the pressing force applied by the rollers is tightly combined with the carbon fiber woven cloth pre-placed through the rollers to obtain a carbon fiber reinforced aluminum-based composite plate; wherein, the spacing between the rollers is 4mm, and the rolling speed is 3r / min-5r / min.

[0008] The present invention discloses a method for preparing a carbon fiber reinforced aluminum-based composite plate by using a semi-solid casting and rolling method. In step 3, the raw materials for the semi-solid casting and rolling composite are the surface nickel-plated carbon fiber woven cloth obtained in step 1 and the aluminum alloy semi-solid slurry obtained in step 2.

[0009] The key technical point of the present invention is that: the present invention develops a method for preparing a carbon fiber woven cloth reinforced aluminum-based composite plate by using a semi-solid casting and rolling method.

[0010] First, the carbon fiber woven cloth is subjected to surface metallization treatment. By coordinating the process parameters of each phase in the pre-plating treatment and the plating treatment, the carbon fiber woven cloth obtains a complete, uniform and dense nickel-plated layer. Secondly, the semi-solid state is used as the form of aluminum alloy in the composite process. On the one hand, a large amount of latent heat of solidification has been released, which is conducive to the rapid formation of the solid skeleton and ensures the effective transmission of stress in the non-confined space; on the other hand, the aluminum alloy semi-solid slurry has good flowability, which can efficiently fill the fiber voids and provide good protection for the integrity of the fiber organization. Finally, with the mechanical force of the rolling roller, the semi-solid matrix can be forced to continuously infiltrate the nickel-plated carbon fiber woven cloth. During the rolling and infiltration process, the liquid part of the aluminum alloy semi-solid slurry becomes the main filling material inside the infiltrated carbon fiber. Based on the law of interface solute redistribution, the interface organization of carbon fiber-aluminum alloy can be effectively controlled.

[0011] The beneficial effects of the present invention are:

[0012] The present invention applies rolling pressure to the aluminum alloy semi-solid slurry, the top and bottom layers are both aluminum alloy semi-solid slurry (the solid state is suspended in the melt in the form of spherulites), and the middle is nickel-plated carbon fiber woven cloth, so that the aluminum alloy semi-solid slurry performs bilateral synchronous forced infiltration of the nickel-plated carbon fiber woven cloth and forms a strong interface bond, thereby achieving high-quality, short-process preparation of large-size carbon fiber woven cloth reinforced aluminum-based composite plates. The method provided by the present invention can match the corresponding solid phase ratio based on aluminum alloy semi-solid slurries with different components, thereby ensuring the stable distribution and structural integrity of carbon fibers during the casting and rolling process. The prepared carbon fiber woven cloth reinforced aluminum-based composite plate can give full play to the designability of structure and performance, and ensure the lightweight effect of the material to a greater extent.

[0013] The present invention proposes a method for preparing a carbon fiber woven cloth reinforced aluminum-based composite plate by a semi-solid casting and rolling method, which integrates theoretical research and preparation technology, realizes the full infiltration of the aluminum matrix into the carbon fiber, and successfully prepares a composite plate with good combination of the reinforcement phase and the matrix. The present invention has the advantages of simple process, short flow, low price, significant effect, etc., and is expected to provide a feasible way for the large-scale production of such composite materials in my country. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is a schematic diagram of the structure of the device for obtaining the semi-solid slurry of aluminum alloy in the present invention.

[0015] Figure 2It is a schematic diagram of the device of the semi-solid casting and rolling method in the present invention.

[0016] Among them, 1-aluminum alloy semi-solid slurry; 2-stirring paddle; 3-insulation system; 4-carbon fiber preheating system; 5-nickel-plated carbon fiber woven cloth; 6-temperature measurement system; 7-roller; 8-runner; 9-casting nozzle. DETAILED DESCRIPTION

[0017] The method for preparing a carbon fiber reinforced aluminum-based composite plate by a semi-solid casting and rolling method of the present invention is applicable to the following embodiments, but is not limited to the following embodiments.

[0018] The present invention adopts a semi-solid casting and rolling method to cast and roll the carbon fiber woven cloth and the aluminum alloy matrix, wherein the aluminum alloy semi-solid slurry stirring device is as follows Figure 1 As shown, the device comprises a heat preservation system 3 and a stirring paddle 2, and is used to prepare an aluminum alloy semi-solid slurry 1. The aluminum alloy semi-solid slurry and the carbon fiber woven cloth casting and rolling device are as shown in FIG. Figure 2 As shown, it is composed of a roller 7, a casting nozzle 9, a runner 8, a heat preservation system 3, a temperature measurement system 6 and a carbon fiber preheating system 4. The heat preservation system 3 is on both sides of the runner 8 to ensure that the temperature before casting is between the solid-liquid two-phase region; the temperature measurement system 6 measures the real-time temperature of the aluminum alloy semi-solid slurry 1 at the runner; the nickel-plated carbon fiber woven cloth 5 first passes through the carbon fiber preheating system 4 and then passes through the runner 8 in parallel. After the aluminum alloy semi-solid slurry 1 fills the runner, the aluminum alloy semi-solid slurry 1 is subjected to rolling pressure under the mechanical pressure of the roller 7. During the pressing process, the uppermost and lowermost layers are both aluminum alloy semi-solid slurry 1 (the solid state is suspended in the melt in the form of spherulites), and the middle is nickel-plated carbon fiber woven cloth, so that the aluminum alloy semi-solid slurry 1 is forced to infiltrate the nickel-plated carbon fiber woven cloth, and a strong interface bond is formed to achieve casting.

[0019] In the method provided by the present invention, the aluminum alloy semi-solid slurry is directly transformed from a semi-solid state to a solid state by the combined effect of the quenching and pressure provided by the rolling rollers, and while rapidly solidifying, the aluminum alloy semi-solid slurry simultaneously penetrates into the interior of the carbon fiber cloth from the upper and lower sides to achieve a firm bond with the carbon fiber cloth.

[0020] In the method for preparing a carbon fiber woven cloth reinforced aluminum-based composite plate by using a semi-solid casting and rolling method provided by the present invention, the aluminum alloy raw material is selected and prepared according to the needs.

[0021] The technical solution of the present invention will be further described below with reference to the accompanying drawings using commercial aluminum alloy ingots of different grades as raw materials.

[0022] Embodiment 1:

[0023] In this embodiment, a carbon fiber woven cloth reinforced aluminum-based composite plate is prepared using 2024 aluminum alloy as a matrix, and the steps are as follows:

[0024] Step 1: Metallization of the surface of the carbon fiber woven cloth.

[0025] Step 1.1. Surface glue removal: In an atmospheric environment, burn the carbon fiber woven fabric at 450℃-500℃ for 30min-45min.

[0026] Step 1.2. Surface degreasing: Use a mixture containing 55g / L-65g / L NaOH, 15g / L-25g / L Na 2 CO 3 and 35g / L-45g / L Na 3 PO 4 A ternary alkaline aqueous solution of 70℃-80℃ is used as a degreasing agent, and the carbon fiber woven fabric after degumming is degreased for 20min-40min under the action of ultrasonic vibration, and then the degreased carbon fiber woven fabric is cleaned until there is no degreasing agent residue on the surface.

[0027] Step 1.3. Surface etching: using 50g / L-70g / L H 2 SO 4 、200g / L-300g / L(NH 4 ) 2 S 2 O 8 A 40℃-60℃ aqueous solution is used as an etchant, and the carbon fiber woven fabric after surface degreasing is etched for 15min-20min under the action of ultrasonic vibration, and then the etched carbon fiber woven fabric is cleaned until there is no etchant residue on the surface.

[0028] Step 1.4. Surface sensitization: Place the etched carbon fiber weave in a 30℃-40℃ solution containing 10g / L-20g / L SnCl 2 And 30mL / L-40mL / L HCl sensitizing solution for 25min-30min ultrasonic vibration treatment to form a uniform layer of Sn on its surface 2 (OH) 3 Cl adsorption layer, and then clean the surface sensitized carbon fiber woven cloth until there is no sensitizing liquid residue on the surface.

[0029] Step 1.5. Surface activation: using 0.5g / L-1g / L PdCl 2 , 10mL / L-20mL / L HCl aqueous solution is used as the activation solution, and the surface sensitized carbon fiber woven fabric is activated for 25min-30min at a temperature of 50℃-70℃, and then the activated carbon fiber woven fabric is cleaned until there is no activation solution residue on the surface.

[0030] Step 1.6. Surface deposition: 15g / L-20g / L NiSO 4 6H2 O as main salt, 15g / L-20g / LNaH 2 PO 2 ·H 2 O as a reducing agent, 15mL / L-20mL / L lactic acid as a stabilizer, and 1g / L-3g / L sodium dodecylbenzene sulfonate as a dispersant, and deposition is performed for 30min-120min at pH=3.5-4.5 and 70℃-80℃ to obtain a surface nickel-plated carbon fiber woven cloth.

[0031] Step 2: Preparation of semi-solid aluminum alloy matrix.

[0032] Step 2.1. Material selection: Select commercial 2024 aluminum alloy ingot.

[0033] Step 2.2. Melting: The aluminum alloy ingot is melted in a high-frequency induction furnace, and after being completely melted, it is stirred evenly with a graphite stirring paddle to obtain aluminum alloy liquid. The melting temperature is 700°C.

[0034] Step 2.3. Preparation of aluminum alloy semi-solid slurry: After refining and degassing the aluminum alloy liquid obtained in step 2.2, a graphite stirring paddle is used to stir the aluminum alloy semi-solid slurry with a solid phase ratio of 35%, and then the stirring is stopped and waiting for casting. The stirring speed of the mechanical stirring is 1500r / min, and the stirring time depends on the specific cooling rate.

[0035] Step 3: Semi-solid casting and rolling of the nickel-plated carbon fiber woven cloth and the aluminum alloy matrix.

[0036] Step 3.1. Preheat the surface nickel-plated carbon fiber woven cloth to 350°C-400°C in a thermal resistance furnace, introduce it into the front insulation chamber of the casting and rolling mill, pass it through the center of the roller, and put it in a tensioned state.

[0037] Step 3.2. Use a flat-injection double-roll casting and rolling equipment. The aluminum alloy semi-solid slurry prepared in step 2 is introduced into the insulation chamber in front of the casting and rolling machine. After the temperature is measured by the temperature measuring system, the casting and rolling begins. After the aluminum alloy semi-solid slurry passes through the guide groove and the casting nozzle, it enters between the rollers from the insulation chamber, so that the upper and lower layers of the nickel-plated carbon fiber woven cloth are both aluminum alloy semi-solid slurry. The pressing force applied by the rollers is tightly combined with the carbon fiber woven cloth placed through the rollers in advance, and the aluminum alloy semi-solid slurry is directly transformed from semi-solid to solid to obtain a carbon fiber reinforced aluminum-based composite plate. Among them, the spacing between the rollers is 4mm, and the rolling speed is 4r / min.

[0038] Embodiment 2:

[0039] In this embodiment, a carbon fiber woven cloth reinforced aluminum-based composite plate is prepared using 5083 aluminum alloy as a matrix, and the steps are as follows:

[0040] Step 1: Metallization of the surface of the carbon fiber woven cloth.

[0041] Step 1.1. Surface glue removal: In an atmospheric environment, burn the carbon fiber woven fabric at 450℃-500℃ for 30min-45min.

[0042] Step 1.2. Surface degreasing: Use a mixture containing 55g / L-65g / L NaOH, 15g / L-25g / L Na 2 CO 3 and 35g / L-45g / L Na 3 PO 4 A ternary alkaline aqueous solution of 70℃-80℃ is used as a degreasing agent, and the carbon fiber woven fabric after degumming is degreased for 20min-40min under the action of ultrasonic vibration, and then the degreased carbon fiber woven fabric is cleaned until there is no degreasing agent residue on the surface.

[0043] Step 1.3. Surface etching: using 50g / L-70g / L H 2 SO 4 、200g / L-300g / L(NH 4 ) 2 S 2 O 8 A 40℃-60℃ aqueous solution is used as an etchant, and the carbon fiber woven fabric after surface degreasing is etched for 15min-20min under the action of ultrasonic vibration, and then the etched carbon fiber woven fabric is cleaned until there is no etchant residue on the surface.

[0044] Step 1.4. Surface sensitization: Place the etched carbon fiber weave in a 30℃-40℃ solution containing 10g / L-20g / L SnCl 2 And 30mL / L-40mL / L HCl sensitizing solution for 25min-30min ultrasonic vibration treatment to form a uniform layer of Sn on its surface 2 (OH) 3 Cl adsorption layer, and then clean the surface sensitized carbon fiber woven cloth until there is no sensitizing liquid residue on the surface.

[0045] Step 1.5. Surface activation: using 0.5g / L-1g / L PdCl 2 , 10mL / L-20mL / L HCl aqueous solution is used as the activation solution, and the surface sensitized carbon fiber woven fabric is activated for 25min-30min at a temperature of 50℃-70℃, and then the activated carbon fiber woven fabric is cleaned until there is no activation solution residue on the surface.

[0046] Step 1.6. Surface deposition: 15g / L-20g / L NiSO 4 6H2 O as main salt, 15g / L-20g / LNaH 2 PO 2 ·H 2 O as a reducing agent, 15mL / L-20mL / L lactic acid as a stabilizer, and 1g / L-3g / L sodium dodecylbenzene sulfonate as a dispersant, and deposition is performed for 30min-120min at pH=3.5-4.5 and 70℃-80℃ to obtain a surface nickel-plated carbon fiber woven cloth.

[0047] Step 2: Preparation of semi-solid aluminum alloy matrix.

[0048] Step 2.1 Material selection: Select commercial 5083 aluminum alloy ingot.

[0049] Step 2.2 Melting: The aluminum alloy ingot is melted in a high-frequency induction furnace, and after being completely melted, it is stirred evenly with a graphite stirring paddle to obtain aluminum alloy liquid. The melting temperature is 680°C.

[0050] Step 2.3 Preparation of aluminum alloy semi-solid slurry: After refining and degassing the aluminum alloy liquid obtained in step 2.2, a graphite stirring paddle is used to stir to obtain an aluminum alloy semi-solid slurry with a solid phase ratio of 30%, and then the stirring is stopped and waiting for casting and rolling. The stirring speed of the mechanical stirring is 1500r / min, and the stirring time depends on the specific cooling rate.

[0051] Step 3: Semi-solid casting and rolling of the nickel-plated carbon fiber woven cloth and the aluminum alloy matrix.

[0052] Step 3.1 The surface nickel-plated carbon fiber woven cloth is preheated to 350°C-400°C in a thermal resistance furnace, introduced into the front insulation chamber of the casting and rolling mill, and passed through the center of the roller to be in a tensioned state.

[0053] Step 3.2: Use a flat-injection twin-roll casting and rolling equipment. The aluminum alloy semi-solid slurry prepared in step 2 is introduced into the insulation chamber in front of the casting and rolling machine. After the temperature is measured by the temperature measuring system, the casting and rolling begins. After the aluminum alloy semi-solid slurry passes through the guide groove and the casting nozzle, it enters between the rollers from the insulation chamber, so that the upper and lower layers of the nickel-plated carbon fiber woven cloth are both aluminum alloy semi-solid slurry. The pressing force applied by the rollers is tightly combined with the carbon fiber woven cloth placed through the rollers in advance, and the aluminum alloy semi-solid slurry is directly transformed from semi-solid to solid to obtain a carbon fiber reinforced aluminum-based composite plate. Among them, the spacing between the rollers is 4mm, and the rolling speed is 4r / min.

[0054] Embodiment 3:

[0055] In this embodiment, 4A01 aluminum alloy is used as a matrix to prepare a carbon fiber woven cloth reinforced aluminum-based composite plate, and the steps are as follows:

[0056] Step 1: Metallization of the surface of the carbon fiber woven cloth.

[0057] Step 1.1 Surface glue removal: In an atmospheric environment, burn the carbon fiber woven fabric at 450℃-500℃ for 30min-45min.

[0058] Step 1.2 Surface degreasing: Use a mixture containing 55g / L-65g / L NaOH, 15g / L-25g / L Na 2 CO 3 and 35g / L-45g / L Na 3 PO 4 A ternary alkaline aqueous solution of 70℃-80℃ is used as a degreasing agent, and the carbon fiber woven fabric after degumming is degreased for 20min-40min under the action of ultrasonic vibration, and then the degreased carbon fiber woven fabric is cleaned until there is no degreasing agent residue on the surface.

[0059] Step 1.3 Surface etching: using 50g / L-70g / L H 2 SO 4 、200g / L-300g / L(NH 4 ) 2 S 2 O 8 A 40℃-60℃ aqueous solution is used as an etchant, and the carbon fiber woven fabric after surface degreasing is etched for 15min-20min under the action of ultrasonic vibration, and then the etched carbon fiber woven fabric is cleaned until there is no etchant residue on the surface.

[0060] Step 1.4 Surface sensitization: Place the etched carbon fiber weave in a 30℃-40℃ solution containing 10g / L-20g / L SnCl 2 And 30mL / L-40mL / L HCl sensitizing solution for 25min-30min ultrasonic vibration treatment to form a uniform layer of Sn on its surface 2 (OH) 3 Cl adsorption layer, and then clean the surface sensitized carbon fiber woven cloth until there is no sensitizing liquid residue on the surface.

[0061] Step 1.5 Surface activation: 0.5 g / L-1 g / L PdCl 2 , 10mL / L-20mL / L HCl aqueous solution is used as the activation solution, and the surface sensitized carbon fiber woven fabric is activated for 25min-30min at a temperature of 50℃-70℃, and then the activated carbon fiber woven fabric is cleaned until there is no activation solution residue on the surface.

[0062] Step 1.6 Surface deposition: 15g / L-20g / L NiSO 4 6H2 O as main salt, 15g / L-20g / LNaH 2 PO 2 ·H 2 O as a reducing agent, 15mL / L-20mL / L lactic acid as a stabilizer, and 1g / L-3g / L sodium dodecylbenzene sulfonate as a dispersant, and deposition is performed for 30min-120min at pH=3.5-4.5 and 70℃-80℃ to obtain a surface nickel-plated carbon fiber woven cloth.

[0063] Step 2: Preparation of semi-solid aluminum alloy matrix.

[0064] Step 2.1 Material selection: Select commercial 4A01 aluminum alloy ingot.

[0065] Step 2.2 Melting: The aluminum alloy ingot is melted in a high-frequency induction furnace, and after complete melting, it is stirred evenly with a graphite stirring paddle to obtain aluminum alloy liquid. The melting temperature is 710°C.

[0066] Step 2.3 Preparation of aluminum alloy semi-solid slurry: After refining and degassing the aluminum alloy liquid obtained in step 2.2, a graphite stirring paddle is used to stir to obtain an aluminum alloy semi-solid slurry with a solid phase ratio of 25%, and then the stirring is stopped and waiting for casting and rolling. The stirring speed of the mechanical stirring is 1500r / min, and the stirring time depends on the specific cooling rate.

[0067] Step 3: Semi-solid casting and rolling of the nickel-plated carbon fiber woven cloth and the aluminum alloy matrix.

[0068] Step 3.1 The surface nickel-plated carbon fiber woven cloth is preheated to 350°C-400°C in a thermal resistance furnace, introduced into the front insulation chamber of the casting and rolling mill, and passed through the center of the roller to be in a tensioned state.

[0069] Step 3.2: Use a flat-injection twin-roll casting and rolling equipment. The aluminum alloy semi-solid slurry prepared in step 2 is introduced into the insulation chamber in front of the casting and rolling machine. After the temperature is measured by the temperature measuring system, the casting and rolling begins. After the aluminum alloy semi-solid slurry passes through the guide groove and the casting nozzle, it enters between the rollers from the insulation chamber, so that the upper and lower layers of the nickel-plated carbon fiber woven cloth are both aluminum alloy semi-solid slurry. The pressing force applied by the rollers is tightly combined with the carbon fiber woven cloth placed through the rollers in advance, and the aluminum alloy semi-solid slurry is directly transformed from semi-solid to solid to obtain a carbon fiber reinforced aluminum-based composite plate. Among them, the spacing between the rollers is 4mm, and the rolling speed is 4r / min.

[0070] Embodiment 4:

[0071] In this embodiment, a carbon fiber woven cloth reinforced aluminum-based composite plate is prepared using 3003 aluminum alloy as a matrix, and the steps are as follows:

[0072] Step 1: Metallization of the surface of the carbon fiber woven cloth.

[0073] Step 1.1 Surface glue removal: In an atmospheric environment, burn the carbon fiber woven fabric at 450℃-500℃ for 30min-45min.

[0074] Step 1.2 Surface degreasing: Use a mixture containing 55g / L-65g / L NaOH, 15g / L-25g / L Na 2 CO 3 and 35g / L-45g / L Na 3 PO 4 A ternary alkaline aqueous solution of 70℃-80℃ is used as a degreasing agent, and the carbon fiber woven fabric after degumming is degreased for 20min-40min under the action of ultrasonic vibration, and then the degreased carbon fiber woven fabric is cleaned until there is no degreasing agent residue on the surface.

[0075] Step 1.3 Surface etching: using 50g / L-70g / L H 2 SO 4 、200g / L-300g / L(NH 4 ) 2 S 2 O 8 A 40℃-60℃ aqueous solution is used as an etchant, and the carbon fiber woven fabric after surface degreasing is etched for 15min-20min under the action of ultrasonic vibration, and then the etched carbon fiber woven fabric is cleaned until there is no etchant residue on the surface.

[0076] Step 1.4 Surface sensitization: Place the etched carbon fiber weave in a 30℃-40℃ solution containing 10g / L-20g / L SnCl 2 And 30mL / L-40mL / L HCl sensitizing solution for 25min-30min ultrasonic vibration treatment to form a uniform layer of Sn on its surface 2 (OH) 3 Cl adsorption layer, and then clean the surface sensitized carbon fiber woven cloth until there is no sensitizing liquid residue on the surface.

[0077] Step 1.5 Surface activation: 0.5 g / L-1 g / L PdCl 2 , 10mL / L-20mL / L HCl aqueous solution is used as the activation solution, and the surface sensitized carbon fiber woven fabric is activated for 25min-30min at a temperature of 50℃-70℃, and then the activated carbon fiber woven fabric is cleaned until there is no activation solution residue on the surface.

[0078] Step 1.6 Surface deposition: 15g / L-20g / L NiSO 4 6H2 O as main salt, 15g / L-20g / LNaH 2 PO 2 ·H 2 O as a reducing agent, 15mL / L-20mL / L lactic acid as a stabilizer, and 1g / L-3g / L sodium dodecylbenzene sulfonate as a dispersant, and deposition is performed for 30min-120min at pH=3.5-4.5 and 70℃-80℃ to obtain a surface nickel-plated carbon fiber woven cloth.

[0079] Step 2: Preparation of semi-solid aluminum alloy matrix.

[0080] Step 2.1 Material selection: Select commercial 3003 aluminum alloy ingot.

[0081] Step 2.2 Melting: The aluminum alloy ingot is melted in a high-frequency induction furnace, and after complete melting, it is stirred evenly with a graphite stirring paddle to obtain aluminum alloy liquid. The melting temperature is 700°C.

[0082] Step 2.3 Preparation of aluminum alloy semi-solid slurry: After refining and degassing the aluminum alloy liquid obtained in step 2.2, a graphite stirring paddle is used to stir to obtain an aluminum alloy semi-solid slurry with a solid phase ratio of 35%, and then the stirring is stopped to wait for casting and rolling. The stirring speed of the mechanical stirring is 1500r / min, and the stirring time depends on the specific cooling rate.

[0083] Step 3: Semi-solid casting and rolling of the nickel-plated carbon fiber woven cloth and the aluminum alloy matrix.

[0084] Step 3.1 The surface nickel-plated carbon fiber woven cloth is preheated to 350°C-400°C in a thermal resistance furnace, introduced into the front insulation chamber of the casting and rolling mill, and passed through the center of the roller to be in a tensioned state.

[0085] Step 3.2: Use a flat-injection twin-roll casting and rolling equipment. The aluminum alloy semi-solid slurry prepared in step 2 is introduced into the insulation chamber in front of the casting and rolling machine. After the temperature is measured by the temperature measuring system, the casting and rolling begins. After the aluminum alloy semi-solid slurry passes through the guide groove and the casting nozzle, it enters between the rollers from the insulation chamber, so that the upper and lower layers of the nickel-plated carbon fiber woven cloth are both aluminum alloy semi-solid slurry. The pressing force applied by the rollers is tightly combined with the carbon fiber woven cloth placed through the rollers in advance, and the aluminum alloy semi-solid slurry is directly transformed from semi-solid to solid to obtain a carbon fiber reinforced aluminum-based composite plate. Among them, the spacing between the rollers is 4mm, and the rolling speed is 4r / min.

[0086] Embodiment 5:

[0087] In this embodiment, a carbon fiber woven cloth reinforced aluminum-based composite plate is prepared using 7075 aluminum alloy as a matrix, and the steps are as follows:

[0088] Step 1: Metallization of the surface of the carbon fiber woven cloth.

[0089] Step 1.1 Surface glue removal: In an atmospheric environment, burn the carbon fiber woven fabric at 450℃-500℃ for 30min-45min.

[0090] Step 1.2 Surface degreasing: Use a mixture containing 55g / L-65g / L NaOH, 15g / L-25g / L Na 2 CO 3 and 35g / L-45g / L Na 3 PO 4 A ternary alkaline aqueous solution of 70℃-80℃ is used as a degreasing agent, and the carbon fiber woven fabric after degumming is degreased for 20min-40min under the action of ultrasonic vibration, and then the degreased carbon fiber woven fabric is cleaned until there is no degreasing agent residue on the surface.

[0091] Step 1.3 Surface etching: using 50g / L-70g / L H 2 SO 4 、200g / L-300g / L(NH 4 ) 2 S 2 O 8 A 40℃-60℃ aqueous solution is used as an etchant, and the carbon fiber woven fabric after surface degreasing is etched for 15min-20min under the action of ultrasonic vibration, and then the etched carbon fiber woven fabric is cleaned until there is no etchant residue on the surface.

[0092] Step 1.4 Surface sensitization: Place the etched carbon fiber weave in a 30℃-40℃ solution containing 10g / L-20g / L SnCl 2 And 30mL / L-40mL / L HCl sensitizing solution for 25min-30min ultrasonic vibration treatment to form a uniform layer of Sn on its surface 2 (OH) 3 Cl adsorption layer, and then clean the surface sensitized carbon fiber woven cloth until there is no sensitizing liquid residue on the surface.

[0093] Step 1.5 Surface activation: 0.5 g / L-1 g / L PdCl 2 , 10mL / L-20mL / L HCl aqueous solution is used as the activation solution, and the surface sensitized carbon fiber woven fabric is activated for 25min-30min at a temperature of 50℃-70℃, and then the activated carbon fiber woven fabric is cleaned until there is no activation solution residue on the surface.

[0094] Step 1.6 Surface deposition: 15g / L-20g / L NiSO 4 6H2 O as main salt, 15g / L-20g / LNaH 2 PO 2 ·H 2 O as a reducing agent, 15mL / L-20mL / L lactic acid as a stabilizer, and 1g / L-3g / L sodium dodecylbenzene sulfonate as a dispersant, and deposition is performed for 30min-120min at pH=3.5-4.5 and 70℃-80℃ to obtain a surface nickel-plated carbon fiber woven cloth.

[0095] Step 2: Preparation of semi-solid aluminum alloy matrix.

[0096] Step 2.1 Material selection: Select commercial 7075 aluminum alloy ingot.

[0097] Step 2.2 Melting: The aluminum alloy ingot is melted in a high-frequency induction furnace, and after being completely melted, it is stirred evenly with a graphite stirring paddle to obtain aluminum alloy liquid. The melting temperature is 680°C.

[0098] Step 2.3 Preparation of aluminum alloy semi-solid slurry: After refining and degassing the aluminum alloy liquid obtained in step 2.2, a graphite stirring paddle is used to stir to obtain an aluminum alloy semi-solid slurry with a solid phase ratio of 40%, and then the stirring is stopped to wait for casting and rolling. The stirring speed of the mechanical stirring is 1500r / min, and the stirring time depends on the specific cooling rate.

[0099] Step 3: Semi-solid casting and rolling of the nickel-plated carbon fiber woven cloth and the aluminum alloy matrix.

[0100] Step 3.1 The surface nickel-plated carbon fiber woven cloth is preheated to 350°C-400°C in a thermal resistance furnace, introduced into the front insulation chamber of the casting and rolling mill, and passed through the center of the roller to be in a tensioned state.

[0101] Step 3.2: Use a flat-injection twin-roll casting and rolling equipment. The aluminum alloy semi-solid slurry prepared in step 2 is introduced into the insulation chamber in front of the casting and rolling machine. After the temperature is measured by the temperature measuring system, the casting and rolling begins. After the aluminum alloy semi-solid slurry passes through the guide groove and the casting nozzle, it enters between the rollers from the insulation chamber, so that the upper and lower layers of the nickel-plated carbon fiber woven cloth are both aluminum alloy semi-solid slurry. The pressing force applied by the rollers is tightly combined with the carbon fiber woven cloth placed through the rollers in advance, and the aluminum alloy semi-solid slurry is directly transformed from semi-solid to solid to obtain a carbon fiber reinforced aluminum-based composite plate. Among them, the spacing between the rollers is 4mm, and the rolling speed is 4r / min.

[0102] In a method for preparing a carbon fiber reinforced aluminum-based composite plate material by a semi-solid casting and rolling method provided by the present invention, a carbon fiber woven cloth is selected as the reinforcing phase instead of a unidirectional carbon fiber, thereby avoiding the problem of uneven distribution of the carbon fiber caused by the flow of the aluminum alloy semi-solid slurry during semi-solid casting and rolling, and ensuring that the mechanical properties of the plate material after casting and rolling are equivalent in the warp and weft directions. At the same time, in the present invention, the surface of the carbon fiber is nickel-plated to achieve surface metallization, and the nickel plating treatment solves the problem of insufficient wettability between the surface of the carbon fiber woven cloth and the aluminum alloy semi-solid slurry. At the same time, the nickel plating has more excellent oxidation resistance at high temperatures, is not prone to peeling or degradation, and can effectively ensure the structural integrity and stable distribution of the carbon fiber woven cloth. Based on the aluminum alloy semi-solid slurry, the present invention simultaneously infiltrates and compounds the tensioned carbon fiber woven cloth from both sides, thereby achieving high-quality, short-process, and continuous preparation of the carbon fiber woven cloth reinforced aluminum-based composite plate material.

Claims

1. A method for preparing a carbon fiber cloth reinforced aluminum-based composite plate by semi-solid casting and rolling, characterized in that: The carbon fiber cloth is a carbon fiber woven cloth, and the method comprises the following steps: Step 1: Surface metallization of carbon fiber woven cloth: Step 1.

1. Surface glue removal: Burn the carbon fiber woven cloth in an atmospheric environment; Step 1.

2. Surface degreasing: Using a ternary alkaline aqueous solution as a degreasing agent, the carbon fiber woven fabric after degumming is subjected to a degreasing treatment in the degreasing agent for 20 minutes to 40 minutes under the action of ultrasonic vibration, and then the degreasing carbon fiber woven fabric is cleaned until there is no degreasing agent residue on the surface; Step 1.

3. Surface etching: After the degreased carbon fiber woven fabric is ultrasonically treated in an etchant at 40°C-60°C, the etchant is etched for 15min-20min, and then the etched carbon fiber woven fabric is cleaned until there is no etchant residue on the surface; Step 1.

4. Surface sensitization: Place the etched carbon fiber woven fabric in a sensitizing solution at 30℃-40℃ for 25min-30min ultrasonic vibration treatment to form a uniform Sn2(OH)3Cl adsorption layer on the surface of the carbon fiber woven fabric. Then, clean the surface sensitized carbon fiber woven fabric until there is no sensitizing solution residue on the surface. Step 1.

5. Surface activation: Activate the surface-sensitized carbon fiber woven fabric at 50°C-70°C for 25min-30min, and then wash the activated carbon fiber woven fabric until no activation liquid remains on the surface; Step 1.

6. Surface deposition: depositing the activated carbon fiber woven fabric in a plating solution to obtain a surface nickel-plated carbon fiber woven fabric; Step 2: Preparation of semi-solid aluminum alloy matrix: Step 2.

1. Material selection: Select aluminum alloy raw materials with corresponding components according to needs; Step 2.

2. Melting: Use an induction furnace to melt the aluminum alloy raw material, and stir it evenly with a graphite stirring paddle after it is completely melted to obtain the corresponding aluminum alloy liquid; Step 2.

3. Preparation of semi-solid aluminum alloy slurry: The aluminum alloy liquid obtained in step 2.2 is subjected to refining and degassing treatment, and then cooled, and then mechanical stirring is applied and the temperature is continued to be cooled, and after obtaining a semi-solid aluminum alloy slurry with a solid phase ratio of 25%-40%, stirring is stopped, and the slurry is kept warm and waits for casting and rolling; wherein, the stirring speed of the mechanical stirring is 1500r / min, and the stirring time depends on the specific cooling rate; Step 3: Semi-solid casting and rolling of nickel-plated carbon fiber woven cloth and aluminum alloy matrix: Step 3.

1. Preheat the surface of the nickel-plated carbon fiber woven cloth, introduce it into the front insulation chamber of the casting and rolling mill, pass it through the center of the roller, and put it in a tensioned state; Step 3.

2. Use a flat-injection twin-roll casting and rolling equipment; introduce the aluminum alloy semi-solid slurry into the insulation chamber in front of the casting and rolling machine, and start casting and rolling after the temperature is measured by the temperature measuring system; after the aluminum alloy semi-solid slurry passes through the guide groove and the casting nozzle, it enters between the rollers from the insulation chamber, and the upper and lower layers of the nickel-plated carbon fiber woven cloth are both aluminum alloy semi-solid slurry, which is tightly combined with the carbon fiber woven cloth pre-placed through the rollers through the pressing force applied by the rollers, and the aluminum alloy semi-solid slurry is directly transformed from semi-solid to solid to obtain a carbon fiber reinforced aluminum-based composite plate; wherein, the spacing between the rollers is 4mm, and the rolling speed is 3r / min-5r / min.

2. The method for preparing a carbon fiber cloth reinforced aluminum-based composite sheet by semi-solid casting and rolling according to claim 1, characterized in that: The ternary alkaline aqueous solution contains 55g / L-65g / L NaOH, 15g / L-25g / L Na2CO3 and 35g / L-45g / L Na3PO4; The etchant is an aqueous solution containing 50g / L-70g / L H2SO4 and 200g / L-300g / L (NH4)2S2O8; The sensitizing solution contains 10g / L-20g / L SnCl2 and 30mL / L-40mL / L HCl; The activation solution is an aqueous solution containing 0.5g / L-1g / L PdCl2 and 10mL / L-20mL / L HCl; The plating solution contains 15g / L-20g / L NiSO4·6H2O as the main salt, 15g / L-20g / L NaH2PO2·H2O as the reducing agent, 15mL / L-20mL / L lactic acid as the stabilizer, and 1g / L-3g / L sodium dodecylbenzene sulfonate as the dispersant.

3. The method for preparing a carbon fiber cloth reinforced aluminum-based composite sheet by semi-solid casting and rolling according to claim 1, characterized in that: In step 1.1, the calcination temperature is 450°C-500°C, and the calcination time is 30min-45min.

4. The method for preparing a carbon fiber cloth reinforced aluminum-based composite plate by semi-solid casting and rolling according to claim 1, characterized in that: In step 1.6, during the deposition process, pH = 3.5-4.5, temperature is 70°C-80°C, and deposition time is 30min-120min.

5. The method for preparing a carbon fiber cloth reinforced aluminum-based composite plate by semi-solid casting and rolling method according to claim 1, characterized in that: In step 2.2, the melting temperature is 40°C-60°C higher than the liquidus of the aluminum alloy ingot.

6. The method for preparing a carbon fiber cloth reinforced aluminum-based composite plate by semi-solid casting and rolling method according to claim 1, characterized in that: In step 2.3, stirring is started when the temperature of the aluminum alloy liquid is cooled to 10°C above the melting point.

7. The method for preparing a carbon fiber cloth reinforced aluminum-based composite plate by semi-solid casting and rolling method according to claim 1, characterized in that: In step 3.1, the preheating temperature is 350°C-400°C.

Citation Information

Patent Citations

  • Long carbon fiber and metal composite continuous casting machine and process

    CN104493113A

  • Solid-liquid cast-rolling compounding device and method for producing reticular reinforcement interlayer composite material

    CN105290352A

  • Semi-solid die-casting aluminum alloy material and die-casting molding method using same

    CN105525158A

  • Preparation method and cast rolling method of reticular carbon fiber aluminum-based composite material

    CN113897562A