Al3Ti, TiN and AlN reinforced 2024Al composite material with spine-like quasi-continuous net structure and preparation method thereof
By using the spine-like quasi-continuous mesh structure (Al3Ti-AlN-TiN)/2024Al composite material preparation method in aluminum-based composite materials, the problem of decreasing strength of aluminum-based composite materials at high temperatures is solved, and excellent room temperature and high temperatures are achieved Strong plastic matching, simple process and low cost.
Patent Information
- Application Number
- CN202411024176.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
The strength of conventional aluminum-based composite materials decreases due to grain boundary diffusion and plastic rheology at high temperatures. The existing methods are limited by reinforced body pinning, but lead to a decrease in strong plastic matching at room temperature. In situ self-generating reactions are difficult to control the particle size and distribution of reinforced body.
The preparation method of (Al3Ti-AlN-TiN)/2024Al composite material with a spinal quasi-continuous mesh structure is adopted to form a stable "core-shell" structure through ball milling, and the mesh structure is retained in combination with the hot pressing sintering process to regulate Ti2AlN and Al3Ti. The distribution of TiN and AlN forms a multi-scale and multi-level reinforcement skeleton.
It has achieved excellent room temperature strong plastic matching and high temperature stability of aluminum-based composite materials, with a room temperature tensile strength up to 470MPa, and a high temperature tensile strength up to 172MPa at 400℃, and a simple process and low cost.
Smart Images

Figure CN118951008A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an (Al3Ti-AlN-TiN) / 2024Al composite material with a quasi-vertebral quasi-continuous network structure and a preparation method thereof. Background Art
[0002] Grain boundary diffusion, migration and grain rotation under the combined action of high temperature and external load cause the lattice strain of aluminum grains to be difficult to activate, which is the main reason for limiting the use of conventional aluminum-based composite materials as core structural components at high temperatures. Conventional solution is to use enough reinforcements to pin grains, limit plastic rheology at high temperatures, and thus maintain high temperature strength. However, too many reinforcements are very easy to reunite, which seriously damages the matching of normal temperature strong plasticity. It is mentioned in CN110747378A that as the reinforcement (Ti3AlC2 and Al3Ti) content in the composite material is increased from 13.3vol.% to 55.3vol.%, the normal temperature strong plasticity is weakened from 207MPa and 4.1% to 200MPa and 1.3%, because the reinforcements reunited cause local stress and strain concentration, causing the composite material to fail prematurely.
[0003] In order to solve this problem, the academic community designed the microstructure from the perspective of classical mechanics and proposed the concept of a "quasi-continuous network structure" in which the reinforcement surrounds the matrix in a quasi-continuous state and the matrix is interconnected. The morphology and distribution of the reinforcement in the network skeleton have a great influence on the bearing and evacuation of stress and strain, and the configuration (thickness, connectivity) of the network skeleton plays a key role in improving the strength-plasticity matching of the quasi-continuous network composite material.
[0004] Ti2AlN is a ternary layered compound ceramic with both covalent bonds and metallic bonds. It reacts with Al at high temperatures to generate multi-scale Al3Ti, TiN and AlN in situ. All three are high-temperature reinforcement phases of great concern in aluminum-based composites. Therefore, it is reasonable to expect that regulating the distribution of Al3Ti, TiN and AlN to achieve quasi-continuous network structures with different configuration parameters will greatly improve the room temperature strength and plasticity matching of composites. In addition, the network structure skeleton has an all-round binding effect on the matrix at high temperatures, which can effectively overcome and constrain the thermal expansion and plastic rheology of the aluminum matrix, and play a role in bearing and strengthening. However, in-situ self-generated reactions usually occur during the preparation process, and it is extremely difficult to intervene in the particle size and distribution of the reinforcement in this process. Therefore, it is difficult to configure the in-situ self-generated reinforcement. Therefore, there has never been a report on the introduction of quasi-continuous network structures into Al3Ti, TiN and AlN reinforced aluminum-based composites. Summary of the invention
[0005] In view of this, the object of the present invention is to provide a method for preparing a (Al3Ti-AlN-TiN) / 2024Al composite material with a quasi-continuous network structure similar to a spine, which is easy to operate and low in cost.
[0006] The present invention also aims to provide a (Al3Ti-AlN-TiN) / 2024Al composite material with a quasi-continuous network structure similar to a spine.
[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0008] According to a first aspect of the present invention, a method for preparing a (Al3Ti-AlN-TiN) / 2024Al composite material having a quasi-continuous network structure is provided, comprising the following steps:
[0009] Step S1, preparing a stable "core-shell" structure composite material powder;
[0010] Step S2, retaining the "core-shell" structure through a reasonable hot pressing sintering process.
[0011] Furthermore, the step S1 comprises:
[0012] Step S11, mixing ingredients according to the volume fraction of the composite material: weigh Ti2AlN powder and 2024Al powder according to the volume ratio, wherein the Ti2AlN content is 3-20 vol.%, and the rest is 2024Al powder;
[0013] Step S12, putting various raw materials weighed in step S11 into a drum ball mill, and ball milling them at a speed of 90 r / min for 5 hours according to a ball-to-material ratio of 5:1, which is regarded as one-step ball milling;
[0014] Step S13, putting the mixed powder of step S12 into a planetary ball mill, and milling at a speed of 150 r / min for 2 h according to a ball-to-material ratio of 5:1, which is regarded as two-step ball milling;
[0015] Furthermore, the step S2 comprises:
[0016] Step S21, laying the mixed powder on the bottom of a graphite mold coated with boron nitride, with a thickness of 25 to 30 mm, and cold pressing to obtain the green body;
[0017] Step S22, sintering the green body obtained in S21 in a high-purity argon atmosphere, with a sintering temperature of 700-730°C, a heating rate of 10°C / min, and a holding time of 30min; then cooling it to 590°C with the furnace, pressurizing it to 30MPa, and keeping it at this temperature and pressure for 30min; cooling it to room temperature with the furnace and releasing the pressure to obtain the green body.
[0018] According to a second aspect of the present invention, there is provided a (Al3Ti-AlN-TiN) / 2024Al composite material with a vertebral-like quasi-continuous network structure prepared by the preparation method of any embodiment of the first aspect.
[0019] The above technical solution of the present invention has at least one of the following beneficial effects:
[0020] According to the preparation method of the present invention, a (Al3Ti-AlN-TiN) / 2024Al composite material with a quasi-continuous network structure similar to a spine is obtained, and its structure is flexible and adjustable. First, the precursor Ti2AlN powder is evenly distributed on the surface of the 2024Al powder particles by one-step ball milling, and the Ti2AlN powder is embedded into the surface of the 2024Al powder particles by two-step ball milling to obtain a stable "core-shell" structure composite material powder, and then, its "core-shell" structure is retained during the sintering process. The Ti2AlN precursor reacts with Al and is converted into in-situ self-generated multi-scale Al3Ti, TiN, and AlN, forming a skeleton of a quasi-continuous network structure similar to a spine. The ridge of the skeleton, Al3Ti, is small and equiaxed (1.85-2.98μm) due to insufficient growth space, and is separated by submicron TiN (225-892nm) transformed from Ti2AlN in situ, thus achieving diffuse distribution; the two sides of the skeleton are adjacent to the matrix, and Al3Ti grows in a needle-like structure, interlacing and suturing the skeleton and the adjacent matrix; nano-scale AlN (40-89nm) is dispersed in the crystal. The strong pinning effect of nanoparticles on dislocation movement and grain boundary slip at the microscopic level, and the strong binding effect of the mesh skeleton on the matrix flow at the macroscopic level, achieve a multi-scale and multi-level strengthening effect on the matrix.
[0021] According to the preparation method of the embodiment of the present invention, the (Al3Ti-AlN-TiN) / 2024Al composite material with a quasi-vertebral quasi-continuous network structure obtained has a room temperature tensile strength of up to 470MPa, an elongation of 6.9%, and a high-temperature tensile strength of up to 172MPa at 400°C. The preparation method adopted by the present invention can flexibly control the network structure configuration within a wider range of raw material ratios and temperatures, thereby obtaining an aluminum-based composite material with good comprehensive performance. The preparation method of the present invention has the remarkable characteristics of simple process, convenient operation, and low cost;
[0022] The (Al3Ti-AlN-TiN) / 2024Al composite material with a quasi-continuous network structure of the present invention has excellent room temperature strength-plasticity matching and high temperature stability, which can open up a new path for the research and development and preparation of advanced aluminum-based composite materials for high-temperature core structural components, and is widely used in automobiles, military industry, aerospace and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1The Ti2AlN (shell) / 2024Al (core) composite powder is shown.
[0024] Figure 2 The scanning electron microscope image of the vertebra-like quasi-continuous network structure (Al3Ti-AlN-TiN) / 2024Al composite material is shown;
[0025] Figure 3 The XRD pattern of the vertebrae-like quasi-continuous network structure (Al3Ti-AlN-TiN) / 2024Al composite material is shown. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the described embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.
[0027] First, the preparation method of the (Al3Ti-AlN-TiN) / 2024Al composite material with a vertebral-like quasi-continuous network structure according to an embodiment of the present invention is described in detail below.
[0028] The method for preparing the (Al3Ti-AlN-TiN) / 2024Al composite material with a quasi-continuous network structure according to an embodiment of the present invention comprises the following steps:
[0029] Step S1, preparing a stable "core-shell" structure composite material powder;
[0030] Step S2, retaining the "core-shell" structure through a reasonable hot pressing sintering process.
[0031] In some embodiments of the present invention, step S1 comprises:
[0032] Step S11, mixing ingredients according to the volume fraction of the composite material: weigh Ti2AlN powder and 2024Al powder according to the volume ratio, wherein the Ti2AlN content is 3-20 vol.%, and the rest is 2024Al powder;
[0033] Step S12, putting various raw materials weighed in step S11 into a drum ball mill, and ball milling them at a speed of 90 r / min for 5 hours according to a ball-to-material ratio of 5:1, which is regarded as one-step ball milling;
[0034] Step S13, putting the mixed powder of step S12 into a planetary ball mill, and milling at a speed of 150 r / min for 2 h according to a ball-to-material ratio of 5:1, which is regarded as two-step ball milling;
[0035] In some embodiments of the present invention, step S2 includes:
[0036] Step S21, laying the mixed powder on the bottom of a graphite mold coated with boron nitride, with a thickness of 25 to 30 mm, and cold pressing to obtain the green body;
[0037] Step S22, sintering the green body obtained in S21 in a high-purity argon atmosphere, with a sintering temperature of 700-730°C, a heating rate of 10°C / min, and a holding time of 30min; then cooling it to 590°C with the furnace, pressurizing it to 30MPa, and keeping it at this temperature and pressure for 30min; cooling it to room temperature with the furnace and releasing the pressure to obtain the green body.
[0038] The following is a further description of the preparation method according to the present invention and the prepared vertebral-like quasi-continuous network structure (Al3Ti-AlN-TiN) / 2024Al composite material in combination with specific examples. The tensile strength test method is based on GB / T228.1-2021.
[0039] Embodiment 1
[0040] (1) Weigh the powder according to the volume ratio of Ti2AlN to 2024Al of 3:97, weigh 1.3g Ti2AlN powder, 27.2g
[0041] 2024Al powder was placed in a ball mill, and agate balls were added at a ball-to-material ratio of 5:1. The ball mill was placed on a drum ball mill and ball milled at a speed of 90 r / min for 5 h to fully mix the powder.
[0042] (2) The ball-milled powder is placed on a planetary ball mill and ball-milled at a speed of 150 r / min for 2 h to embed Ti2AlN into the surface of the Al particles to obtain a "core-shell" structured composite material powder.
[0043] (3) The ball-milled powder is placed in a graphite mold coated with boron nitride and cold-pressed into shape.
[0044] (4) Sintering is performed by hot pressing. The specific process is: in a high-purity argon atmosphere, the temperature is raised to 730°C at a rate of 10°C / min, kept at this temperature for 30 minutes, then cooled to 590°C with the furnace, pressurized to 30MPa, kept at this temperature for 30 minutes, and then cooled to room temperature with the furnace to release the pressure. The vertebral-like quasi-continuous network structure (Al3Ti-AlN-
[0045] TiN) / 2024Al composite material, wherein the thickness of the vertebral skeleton is 8.99 μm and the connectivity is 92.56%. The composite material is subjected to uniaxial tensile test, and the tensile strength at room temperature is 397 MPa and the elongation is 12%.
[0046] Embodiment 2
[0047] (1) Weigh the powder according to the volume ratio of Ti2AlN to Al of 3:97, weigh 1.3g Ti2AlN powder and 27.2g Al powder and place them in a ball mill, and add agate balls according to the ball-to-material ratio of 5:1. Place the ball mill on a drum ball mill and mill at a speed of 90r / min for 5h to fully mix the powder.
[0048] (2) The ball-milled powder is placed on a planetary ball mill and ball-milled at a speed of 150 r / min for 2 h to embed Ti2AlN into the surface of the Al particles to obtain a "core-shell" structured composite material powder.
[0049] (3) The ball-milled powder is placed in a graphite mold coated with boron nitride and cold-pressed into shape.
[0050] (4) Sintering is performed by hot pressing. The specific process is as follows: in a high-purity argon atmosphere, the temperature is raised to 730°C at a rate of 10°C / min, kept at this temperature for 30 minutes, then cooled to 590°C with the furnace, pressurized to 30MPa, kept at this temperature for 30 minutes, and then cooled to room temperature with the furnace to release the pressure. A vertebral-like quasi-continuous network structure (Al3Ti-AlN-TiN) Al composite material is obtained, in which the vertebral-like skeleton has a thickness of 10.06μm and a connectivity of 86.23%. The composite material is subjected to a uniaxial tensile test, and the tensile strength at room temperature is 223MPa and the elongation is 16%.
[0051] Embodiment 3
[0052] (1) Weigh the powder according to the volume ratio of Ti2AlN to Al of 10:95, weigh 4.6g Ti2AlN powder and 26.2g Al powder and place them in a ball mill, and add agate balls according to the ball-to-material ratio of 5:1. Place the ball mill on a drum ball mill and mill at a speed of 90r / min for 5h to fully mix the powder.
[0053] (2) The ball-milled powder is placed in a graphite mold coated with boron nitride and cold-pressed into shape.
[0054] (3) Sintering is performed by hot pressing. The specific process is: in a high-purity argon atmosphere, the temperature is raised to 660°C at a rate of 10°C / min, the pressure is increased to 30MPa, the temperature is maintained for 30 minutes, and the pressure is released after cooling to room temperature. The (Al3Ti-AlN-TiN) / Al composite material is obtained, which has no quasi-continuous network structure characteristics of the vertebrae, has a tensile strength of 233MPa at room temperature, and an elongation of 2.0%.
[0055] Embodiment 4
[0056] (1) Weigh the powder according to the volume ratio of Ti2AlN to 2024Al of 10:90, weigh 4.6g Ti2AlN powder, 26.2g
[0057] 2024Al powder was placed in a ball mill, and agate balls were added at a ball-to-material ratio of 5:1. The ball mill was placed on a drum ball mill and ball milled at a speed of 90 r / min for 10 h to fully mix the powder.
[0058] (2) The ball-milled powder is placed on a planetary ball mill and ball-milled at a speed of 150 r / min for 2 h to embed Ti2AlN into the surface of the Al particles to obtain a "core-shell" structured composite material powder.
[0059] (3) The ball-milled powder is placed in a graphite mold coated with boron nitride and cold-pressed into shape.
[0060] (4) Sintering is performed by hot pressing. The specific process is as follows: in a high-purity argon atmosphere, the temperature is raised to 700°C at a rate of 10°C / min, kept at this temperature for 30 minutes, then cooled to 590°C with the furnace, pressurized to 30MPa, kept at this temperature for 30 minutes, and then cooled to room temperature with the furnace to release the pressure. A quasi-continuous network structure (Al3Ti-AlN-
[0061] TiN) / 2024Al composite material, in which the thickness of the vertebral skeleton is 19.03μm and the connectivity is 84.50%. The composite material was subjected to uniaxial tensile test, and the tensile strength at room temperature was 470MPa and the elongation was 6.9%. At 400℃
[0062] The high temperature strength is 120MPa.
[0063] Embodiment 5
[0064] (1) Weigh the powder according to the volume ratio of Ti2AlN to 2024Al of 20:90, weigh 9.2g Ti2AlN powder and 23.3g 2024Al powder and put them in a ball mill, and add agate balls according to the ball-to-material ratio of 5:1. Place the ball mill on a drum ball mill and mill at a speed of 90r / min for 10h to fully mix the powder.
[0065] (2) The ball-milled powder is placed on a planetary ball mill and ball-milled at a speed of 150 r / min for 2 h to embed Ti2AlN into the surface of the Al particles to obtain a "core-shell" structured composite material powder.
[0066] (3) The ball-milled powder is placed in a graphite mold coated with boron nitride and cold-pressed into shape.
[0067] (4) Sintering is performed by hot pressing. The specific process is as follows: in a high-purity argon atmosphere, the temperature is raised to 700°C at a rate of 10°C / min, kept at this temperature for 30 minutes, then cooled to 590°C with the furnace, pressurized to 30MPa, kept at this temperature for 30 minutes, and then cooled to room temperature with the furnace to release the pressure. A quasi-continuous network structure (Al3Ti-AlN-
[0068] TiN) / 2024Al composite material, in which the thickness of the vertebral skeleton is 25.42μm and the connectivity is 80.13%. The composite material was subjected to uniaxial tensile test, and the tensile strength at room temperature was 356MPa and the elongation was 2%. At 400℃
[0069] The high temperature strength is 172MPa.
[0070] The above are preferred embodiments and comparative examples of the present invention, wherein Examples 1 and 2 are comparative examples to each other, illustrating that the 2024Al matrix can give the composite material a better strength-plasticity match compared to the Al matrix; Examples 3 and 4 are comparative examples to each other, illustrating the necessity of double-step ball milling and the preferred sintering temperature of the present invention for forming a quasi-continuous network structure of the vertebral body. Examples 1, 4, and 5 are preferred embodiments of the present invention, illustrating the proportional relationship between the amount of Ti2AlN added and the thickness of the skeleton of the vertebral network structure of the composite material, and revealing the method for regulating the parameters of the vertebral network structure of the present invention. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, several improvements and modifications can be made, and these improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A (Al3Ti-AlN-TiN) / 2024Al composite material with a quasi-vertebral quasi-continuous network structure, characterized in that: (1) The raw materials are Ti2AlN powder and 2024Al powder, wherein the content of Ti2AlN is 3-20 vol.%, and the rest is 2024Al; (2) A "core-shell" structure composite material powder is obtained by two-step ball milling; (3) The "core-shell" structure is retained by hot pressing and sintering to obtain a (Al3Ti-AlN-TiN) / 2024Al composite material with a quasi-continuous network structure similar to a spine; (4) The skeleton structure is composed of multi-scale Al3Ti, TiN and AlN generated by the reaction of Ti2AlN and Al.
2. The (Al3Ti-AlN-TiN) / 2024Al composite material with a quasi-continuous network structure as claimed in claim 1, characterized in that: The original powder is 2024Al spherical powder with a particle size of 75 to 150 μm and Ti2AlN powder with a particle size of 2 to 5 μm.
3. The (Al3Ti-AlN-TiN) / 2024Al composite material with a vertebral-like quasi-continuous network structure according to claim 1 or 2, characterized in that: The "core-shell" structure composite material powder is composed of Ti2AlN uniformly coated and embedded on the surface of 2024Al spherical powder, and the particle size of the composite material powder is 70-118 μm.
4. The (Al3Ti-AlN-TiN) / 2024Al composite material with a quasi-continuous network structure as described in any one of claims 1 to 3, characterized in that: The vertebral-like skeleton is composed of two morphologies (needle-shaped and equiaxed) of micron-sized Al3Ti (1.85-2.98μm) and submicron-sized TiN (225-892nm); equiaxed Al3Ti and TiN are diffusely distributed in the ridge of the skeleton, and needle-shaped Al3Ti is interspersed on both sides of the ridge to suture the skeleton and the adjacent matrix.
5. The (Al3Ti-AlN-TiN) / 2024Al composite material with a quasi-continuous network structure as described in any one of claims 1 to 4, characterized in that: Nano-scale AlN (40-89 nm) is dispersed inside the matrix grains.
6. The (Al3Ti-AlN-TiN) / 2024Al composite material with a quasi-continuous network structure as described in any one of claims 1 to 5, characterized in that: The skeleton thickness is 8.99-19.03 μm, and the skeleton connectivity is 84.50-92.56%.
7. The method for preparing the (Al3Ti-AlN-TiN) / 2024Al composite material with a quasi-continuous network structure as claimed in any one of claims 1 to 6, characterized in that: The steps include: Step S1, preparing a stable "core-shell" structure composite material powder; Step S2, retaining the "core-shell" structure through a reasonable hot pressing sintering process.
8. The preparation method according to claim 7, characterized in that: The step S1 comprises the following steps: Step S11, mixing ingredients according to the volume fraction of the composite material: weigh Ti2AlN powder and 2024Al powder according to the volume ratio, wherein the Ti2AlN content is 3-20 vol.%, and the rest is 2024Al powder; Step S12, putting various raw materials weighed in step S11 into a drum ball mill, and ball milling them at a speed of 90 r / min for 5 hours according to a ball-to-material ratio of 5:1, which is regarded as one-step ball milling; Step S13, putting the mixed powder of step S12 into a planetary ball mill, and ball milling it at a speed of 150r / min for 2h according to a ball-to-material ratio of 5:1, which is regarded as two-step ball milling, to obtain a stable "core-shell" structure composite material powder.
9. The preparation method according to claim 7, characterized in that: The step S2 comprises the following steps: Step S21, laying the mixed powder on the bottom of a graphite mold coated with boron nitride, with a thickness of 25 to 30 mm, and cold pressing to obtain the green body; Step S22, sintering the green body obtained in S21 in a high-purity argon atmosphere, with a sintering temperature of 700-730°C, a heating rate of 10°C / min, and a holding time of 30min; then cooling it to 590°C with the furnace, pressurizing it to 30MPa, and keeping it at this temperature and pressure for 30min; cooling it to room temperature with the furnace and releasing the pressure to obtain the green body.
10. An (Al3Ti-AlN-TiN) / 2024Al composite material having a vertebral-like quasi-continuous network structure prepared according to the preparation method according to any one of claims 1 to 10.
Citation Information
Patent Citations
Ti3AlC2-Al3Ti biphase reinforced Al-based composite and hot-pressing preparation method thereof
CN110747378A