Method for controlling generation of mirror image laser welding defects through partition targeted regulation and control technology

Through partition targeted control technology, the problems of pores, undercuts, mechanical performance losses and keyhole instability in laser manufacturing are controlled, and the high-performance output of aluminum alloy welding joints in laser mirror welding is achieved, solving the defects in welding process. Problem, significantly reducing welding deformation and defects.

CN118951422AInactive Publication Date: 2024-11-15NANJING UNIV OF AERONAUTICS & ASTRONAUTICS +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410821928.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The problems of pores, undercuts, mechanical performance losses and keyhole instability during laser mirror welding lead to a degradation of the overall performance of aluminum alloy welded joints.

Method used

Through partition targeting control technology, laser energy, prefabricated laser offset, adjust laser energy distribution factor and change laser incidence angle, forming a partition targeting control process window for microscopic defects of laser manufacturing welds, specifically including design process experiments and obtaining data , create energy density models, study asymmetric heat flow transmission behavior, analyze element burn-out models and keyhole comprehensive stress, and then control various defects.

Benefits of technology

Welding deformation is significantly suppressed, lightweight, high-power structural parts with small deformation and few defects are prepared, and the comprehensive performance of aluminum alloy welded joints is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118951422A_ABST
    Figure CN118951422A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of laser manufacturing, discloses a method for controlling generation of mirror image laser welding defects through a partition targeted regulation and control technology, and aims to solve the potential problems of alpha region pore defects, beta region undercut defects, gamma region mechanical property loss and delta region keyhole instability in mirror image laser manufacturing. By using a strategy fed back by field situation awareness and simulation means, accurate transmission of data and model calculation is ensured, accuracy of shape regulation and control is ensured, an accurate zoning targeted regulation and control model process is obtained, and a zoning targeted regulation and control process window for the laser-manufactured weld microdefects is formed; the method comprises the following steps: carrying out defect partition targeted regulation and control by means of controlling laser energy, prefabricating laser offset, adjusting laser energy distribution factors, changing a laser incident angle and the like, controlling pore defects, element burning loss and molten pool stability of a welding joint area, and inhibiting welding deformation vertical to a path direction; and the light high-strength large structural member with small deformation and few defects is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of laser manufacturing technology, and in particular to a method for controlling the generation of mirror laser welding defects through a partitioned targeted control technology. Background Art

[0002] As an advanced connection technology, laser manufacturing technology has become one of the common connection methods for aluminum alloy structural parts due to its advantages such as high energy density and high precision. However, laser manufacturing often welds on one side of the weldment, and the temperature difference between the front and back sides of the weldment is large, which inevitably produces large welding deformation. The laser mirror welding method can achieve deformation-free and high-efficiency welding of the plate, but due to the special welding method of laser mirror welding, the flat plate butt joint structure is subjected to the symmetrical dual laser heat source during the welding process, and there is a complex interaction of double keyholes and double-sided joint molten pools, and the factors affecting the stability of the molten pool during the welding process are significantly increased. Therefore, the present invention proposes a method for controlling the generation of mirror laser welding defects through partitioned targeted control technology, by constructing a laser manufacturing weld micro-defect partitioned targeted control process window, and sequentially controlling the "α zone" porosity defect, "β zone" undercut defect, "γ zone" mechanical property loss and "δ zone" keyhole instability potential problems, thereby solving the problem of defects in the laser mirror welding process, improving the comprehensive performance of aluminum alloy welded joints, and preparing lightweight, high-strength and large-scale structural parts with small deformation and few defects. Summary of the invention

[0003] The purpose of the present invention is to provide a method for controlling the generation of mirror laser welding defects through partition targeted control technology, so as to solve the degradation of comprehensive performance of aluminum alloy welded joints caused by serious defects in laser mirror welding.

[0004] To achieve this object, the present invention adopts the following technical solutions:

[0005] The mirror laser manufacturing potential "α zone" porosity defects, "β zone" undercut defects, "γ zone" mechanical property loss and "δ zone" keyhole instability problems are carried out by controlling laser energy, prefabricated laser offset, adjusting laser energy distribution factor, changing laser incident angle and other means to carry out defect zoning targeted regulation. Forming a laser manufacturing weld micro defect zoning targeted regulation process window specifically includes the following steps:

[0006] Step 1: Design a process experiment, use on-site situation awareness means to obtain data such as the morphology and microstructure of the welded joint under process experiments with different laser energies, laser offsets, laser energy distribution factors, and laser incident angles, and construct a process window for targeted control of micro-defect zoning of laser-made welds;

[0007] Step 2: Create an energy density model based on the welding data obtained from the experimental results of different laser energies, carry out research on the evolution process of pores formed by keyhole instability or annihilation, analyze the influence of different energies on the number and distribution characteristics of pores, reveal the formation process of pores, movement laws and influencing factors, and control the pore defects in the "α zone" by controlling the laser energy;

[0008] Step 3: Study the asymmetric heat transfer behavior of mirror laser manufacturing under gravity drive, and study the prefabricated laser offset to control the "β zone" weld defects;

[0009] Step 4: Create an element burnout model based on the element changes before and after welding obtained from the experimental results. According to the photothermal conversion mechanism and the equilibrium vapor pressure theory, a correlation mechanism between the element burnout and the microstructure is formed. The mechanical property loss in the "γ zone" is suppressed by adjusting the laser energy distribution factor.

[0010] Step 5: Study the comprehensive force analysis of the keyhole. Under the condition of double keyhole coupling penetration, analyze the compression effect of the gravity of the metal above the keyhole on the keyhole, and maintain the stable shape of the keyhole in the "δ zone" by changing the laser incident angle;

[0011] Preferably, the "α zone" pore defects are studied by in-situ visualization of the formation and evolution process of microscopic defects by the laser manufacturing head based on high-precision synchrotron X-ray three-dimensional imaging technology, and the defect morphology, size, quantity and position in the laser manufacturing process are quantitatively characterized. Combined with the simulation results of bubble movement and evolution, the pore morphology, distribution, size and other characteristics under different laser energies are studied, and finally the pore defect problem is controlled by controlling the laser energy.

[0012] Preferably, for the "β zone" undercut defect, the surface morphology of the free molten pool is calculated using the fluid volume function method (VOF), and the orthogonal test method is used to study the influence of different laser powers, welding speeds, and heat source pre-offsets on the macroscopic morphology of the weld, and the inflection points of the weld width on both sides of the weld under different laser offsets are obtained, and the appropriate laser offset is selected to regulate the macroscopic morphology of the weld.

[0013] Preferably, the mechanical property loss of the "γ zone" is calculated, the evaporation area and the remainder of the alloy elements before and after welding are calculated, and the correlation model of element burnout-weld strength loss is derived in turn to obtain the area where the surface temperature is higher than the boiling point of the alloy component elements. Under the premise of ensuring the weld formation, the laser spot size and the energy distribution factor are adjusted to minimize the surface area of ​​the high temperature zone of the molten pool.

[0014] Preferably, the instability problem of the keyhole in the "δ zone" is studied, and the comprehensive force analysis of the keyhole under the condition of double keyhole coupling penetration is studied, and the additional pressure Pσ of the surface tension of the liquid molten pool, the steam pressure Pr generated by the vaporization of the liquid metal, the gravity Pg of the liquid metal on the keyhole wall, the fluid dynamic pressure Pc caused by the flow of the molten pool around the keyhole, the beam pressure Pb generated by the laser beam irradiating the metal surface, the shear force Fs caused by the tangential velocity of the fluid and the tangential force Fσ caused by the surface tension gradient are calculated respectively. The force coupling analysis of the keyhole in the confined micro-molten pool is carried out, focusing on the compression effect of the gravity of the metal above the keyhole on the keyhole, and the stable shape of the keyhole in the "δ zone" is maintained by changing the laser incident angle.

[0015] Compared with the laser manufacturing technology in the prior art, the method of the present invention has the following advantages:

[0016] 1. The mirror laser manufacturing method is adopted so that the residual stress of the conjugate distribution in the welding process can significantly suppress the welding deformation perpendicular to the path direction.

[0017] 2. By adopting the zoned targeted control technology and forming a zoned targeted control process window for laser manufacturing weld micro-defects, large-scale lightweight and high-strength structural parts with small deformation and few defects can be prepared.

[0018] 3. The strategy of on-site situation awareness and simulation feedback is adopted to ensure the accurate transmission of data and model calculations, thus ensuring the accuracy of shape control. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a flow chart of controlling pores and defects by using a partitioned targeted regulation technology provided by a specific embodiment of the present invention;

[0020] Figure 2 It is a schematic diagram of welding defects in each area of ​​the laser mirror welding partition targeted control technology provided by a specific embodiment of the present invention; DETAILED DESCRIPTION

[0021] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the present invention. It should also be noted that, for ease of description, only parts related to the present invention, rather than all structures, are shown in the accompanying drawings.

[0022] The embodiment of the present invention provides a method for controlling the generation of mirror laser welding defects by using a partitioned targeted control technology, such as Figure 1As shown in the figure, for the potential porosity defects in the "α zone", undercut defects in the "β zone", keyhole instability in the "δ zone" and mechanical property loss in the "γ zone" during the mirror-image laser transverse welding of a 2mm thick 2195 aluminum-lithium alloy flat plate, targeted regulation of defect zoning is carried out by controlling laser energy, prefabricating laser offset, changing laser incident angle, and adjusting laser energy distribution factors. A process window for targeted regulation of microscopic defects in laser manufacturing welds is formed.

[0023] Firstly, the process experiment was designed according to the orthogonal variable method. The laser focusing device was clamped by KUKA KR60 welding robot. The laser energy ranged from 1000W to 1600W, increasing by 50W per group of experiments. The morphology and microstructure of the welded joints under different laser energies were obtained. High-precision synchrotron radiation X-ray three-dimensional imaging technology was used to image the dynamics of the molten pool at a frame rate of up to 4KHz and an effective pixel size of 1.1um, revealing the pores formed along the melt trajectory due to the steam recoil force, forming an in-situ visualization study of the evolution of the laser mirror welding molten pool, quantitatively characterizing the defect morphology, size, number and position in the laser manufacturing process of aluminum-lithium alloy, and constructing a mapping law between laser process parameters and the morphology, size and distribution characteristics of internal defects in the material. Based on ANSYS fluid simulation software, a laser mirror welding model was constructed to simulate the evolution process of pores formed by bubbles trapped in the mushy zone, study the stress conditions of pore defects of different sizes and morphologies in the molten pool, explain the dynamic mechanism of bubbles in the molten pool, and reveal the formation and evolution mechanism of defects in the welding process. Based on the above-mentioned synchrotron radiation X-ray three-dimensional imaging data and combined with the simulation results of bubble movement and evolution, the pore morphology, distribution, size and other characteristics under different laser energies are studied, and finally the pore defect problem is controlled by controlling the laser energy.

[0024] Then, based on the above experiments and simulations, the optimal laser energy design for 2mm 2195 aluminum-lithium alloy was obtained from 0 to 20mm. The laser offset experiment was carried out with an experimental increment of 2mm in each group to obtain the data such as the morphology and joint quality of the welded joint under different laser offsets. The fluid volume function method (VOF) of the COMSOL Multiphysics software platform was used to calculate the surface morphology of the free molten pool. The orthogonal experimental method was used to study the influence of different laser powers, welding speeds, and heat source prefabrication offsets on the macroscopic morphology of the weld. The inflection points of the weld width on both sides of the weld under different laser offsets were obtained, and the appropriate laser offset was selected to regulate the macroscopic morphology of the weld.

[0025] Secondly, based on the above experiments and simulations, the optimal laser energy and laser offset design of 2mm 2195 aluminum-lithium alloy are obtained from 0 to 100mm. The experimental laser defocus amount is increased by 5mm per group to obtain the data of element loss and mechanical properties of the welded joint under different laser energy distribution factors. According to the light-heat conversion mechanism and the equilibrium vapor pressure theory, the element burning mechanism of alloy elements under the action of laser beam is explored, the evaporation area and residue of alloy elements before and after welding are calculated, and the correlation model of element burning-weld strength loss is derived in turn to obtain the area where the surface temperature is higher than the boiling point of the alloy component elements. Under the premise of ensuring the weld formation, the laser spot size and energy distribution factor are adjusted to minimize the surface area of ​​the high temperature zone of the molten pool and obtain the laser energy distribution factor value with lower mechanical property loss.

[0026] Finally, based on the above experiments and simulations, the optimal laser energy, laser offset, and laser energy distribution factor design of 2mm 2195 aluminum-lithium alloy are obtained from 0 to 45°. The experimental laser incident angle is increased by 5° each time to obtain the data of the molten pool keyhole force and molten pool flow characteristics of the welding joint under different laser incident angles. Under the condition of double keyhole coupling penetration, the additional pressure Pσ of the liquid molten pool surface tension, the vapor pressure Pr generated by the vaporization of the liquid metal, the gravity Pg of the liquid metal on the keyhole wall, the fluid dynamic pressure Pc caused by the molten pool flow around the keyhole, the beam pressure Pb generated by the laser beam irradiating the metal surface, the shear force Fs caused by the tangential velocity of the fluid, and the tangential force Fσ caused by the surface tension gradient are calculated respectively. The force coupling analysis of the keyhole in the confined micro-molten pool is carried out, focusing on the compression effect of the gravity of the metal above the keyhole on the keyhole, and the stable shape of the keyhole in the "δ zone" is maintained by changing the laser incident angle.

[0027] Finally, the data obtained from the above experiments were used to create a targeted control process window for micro-defect zoning of 2mm thick 2195 aluminum-lithium alloy laser-made welds, which can significantly suppress welding deformation perpendicular to the path direction and produce lightweight, high-strength large-scale structural parts with small deformation and few defects.

[0028] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, various obvious changes, readjustments and substitutions can be made without departing from the protection scope of the present invention. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention shall be included in the protection scope of the claims of the present invention.

Claims

1. A method for controlling the generation of mirror laser welding defects through partition targeted control technology, It is characterized in that The mirror laser manufacturing of potential "α zone" porosity defects, "β zone" undercut defects, "γ zone" mechanical property loss and "δ zone" keyhole instability problems is carried out by controlling laser energy, prefabricating laser offset, adjusting laser energy distribution factor, changing laser incident angle and other means to carry out defect zoning targeted regulation and control, forming a laser manufacturing weld micro defect zoning targeted regulation process window, which specifically includes the following steps: Step 1: Design a process experiment, use on-site situation awareness means to obtain data such as the morphology and microstructure of the welded joint under process experiments with different laser energies, laser offsets, laser energy distribution factors, and laser incident angles, and construct a process window for targeted control of micro-defect zoning of laser-made welds; Step 2: Based on the welding data obtained from the experimental results of different laser energies, an energy density model is created to simulate the evolution process of pores formed by keyhole instability or annihilation. The influence of different energies on the number and distribution characteristics of pores is analyzed to reveal the formation process, movement laws and influencing factors of pores, and to control the pore defects in the "α zone" by controlling the laser energy. Step 3: Study the asymmetric heat transfer behavior of mirror laser manufacturing under gravity drive, and study the prefabricated laser offset to control the "β zone" weld defects; Step 4: Create an element burnout model based on the element changes before and after welding obtained from the experimental results. According to the photothermal conversion mechanism and the equilibrium vapor pressure theory, the correlation mechanism between element burnout and microstructure is formed. The mechanical property loss in the "γ zone" is suppressed by adjusting the laser energy distribution factor. Step 5: Study the comprehensive force analysis of the keyhole. Under the condition of double keyhole coupling penetration, analyze the compression effect of the gravity of the metal above the keyhole on the keyhole, and maintain the stable shape of the keyhole in the "δ zone" by changing the laser incident angle.

2. According to claim 1, a method for controlling the generation of mirror laser welding defects by partition targeted control technology, It is characterized in that The "α zone" pore defects are studied by in-situ visualization of the formation and evolution process of microscopic defects in the laser manufacturing head based on high-precision synchrotron X-ray three-dimensional imaging technology. The defect morphology, size, quantity and position in the laser manufacturing process are quantitatively characterized. Combined with the simulation results of bubble movement and evolution, the pore morphology, distribution, size and other characteristics under different laser energies are studied. Finally, the pore defect problem is controlled by controlling the laser energy.

3. According to claim 1, a method for controlling the generation of mirror laser welding defects by partition targeted control technology, It is characterized in that For the "β zone" undercut defect, the volume function method (VOF) of fluid is used to calculate the surface morphology of the free molten pool, and the orthogonal test method is used to study the influence of different laser powers, welding speeds, and pre-excursion amounts of heat source on the macroscopic morphology of the weld. The inflection points of the weld width on both sides of the weld under different laser offsets are obtained, and the appropriate laser offset is selected to regulate the macroscopic morphology of the weld.

4. According to claim 1, a method for controlling the generation of mirror laser welding defects by partition targeted control technology, It is characterized in that The mechanical property loss of the "γ zone" is calculated, the evaporation area and margin of the alloy elements before and after welding are calculated, and the correlation model of element burnout-weld strength loss is derived in turn to obtain the area where the surface temperature is higher than the boiling point of the alloy component elements. Under the premise of ensuring the formation of the weld, the laser spot size and energy distribution factor are adjusted to minimize the surface area of ​​the high temperature zone of the molten pool.

5. According to claim 1, a method for controlling the generation of mirror laser welding defects by partition targeted control technology, It is characterized in that The instability problem of the keyhole in the "δ zone" is studied, and the comprehensive force analysis of the keyhole under the condition of double keyhole coupling penetration is studied. The additional pressure Pσ of the surface tension of the liquid molten pool, the steam pressure Pr generated by the vaporization of the liquid metal, the gravity Pg of the liquid metal on the keyhole wall, the fluid dynamic pressure Pc caused by the flow of the molten pool around the keyhole, the beam pressure Pb generated by the laser beam irradiating the metal surface, the shear force Fs caused by the tangential velocity of the fluid and the tangential force Fσ caused by the surface tension gradient are calculated respectively. The force coupling analysis of the keyhole in the confined micro-molten pool is carried out, and the compression effect of the gravity of the metal above the keyhole on the keyhole is analyzed in detail. The stable shape of the keyhole in the "δ zone" is maintained by changing the laser incident angle.

Citation Information

Patent Citations

  • Mirror image laser welding device and method for optimizing weld joint forming of molten pool

    CN111545906A

  • Laser mirror welding method

    CN111604593A