By using polymer mesh structure wrapping technology of materials such as epoxy resin and diamond in the grinding sheet, the problems of uneven grinding and low efficiency of marble are solved, and uniform and efficient grinding of marble is achieved and cost reduction of marble is achieved.
Patent Information
- Application Number
- CN202411059294.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-03
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-03
AI Technical Summary
The existing grinding sheets have problems of uneven grinding and low efficiency in the marble grinding process, especially the grinding efficiency and cumbersome steps for traditional hard stones such as granite, concrete, marble, and quartz stone, resulting in high production and use costs.
Using a grinding sheet including epoxy resin, diamond, resin curing agent, mullite, silicon carbide, corundum and wollastonite, a polymer network structure is formed through a specific mixing and heating process, and evenly wraps the diamond powder. Form a grinding sheet with stable performance. The preparation method of the grinding sheet includes initial mixing of epoxy resin with diamond, then adding other materials and stirring in a mixer to form a preliminary mix, then heating and curing in a mold, finally demolding and performing secondary heating to improve Performance of grinding sheets.
It realizes uniform and efficient grinding of marble, improves grinding efficiency and flatness, reduces production and use costs, and the roughness of the grinding sheet is stable at 50 mesh, suitable for marble materials on the market.
Smart Images

Figure CN118952059A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of stone abrasives, in particular to a grinding disc for uniform and efficient grinding of marble and a preparation method thereof. Background Art
[0002] Abrasive discs are tools used for grinding, which fix abrasives in various ways to perform surface treatment on various materials. Abrasive discs have a wide range of applications, including but not limited to stone processing, metal material processing, pulp fiber processing, etc. According to different application scenarios and processing requirements.
[0003] Diamond grinding disc is one of the most commonly used marble polishing grinding discs, which has the characteristics of high hardness, high wear resistance and high efficiency. For example, CN218891731U relates to a soft grinding disc for marble polishing. The utility model achieves the advantages of easy assembly and disassembly of the soft grinding disc and replacement of a single grinding block by setting a grinding block, a mounting column, a limit ring, a connecting column, a first fixed column, a first connecting rod, a second fixed column, a clamping column, a tension spring, a connecting block, a clamping block, a compression spring, a second connecting rod and a button. However, no improvement is made on the grinding disc material, so that the grinding of marble still has the problems of uneven grinding and low grinding efficiency.
[0004] In order to achieve uniform grinding and improve grinding efficiency, a grinding disc for uniform and efficient grinding of marble and a preparation method thereof are proposed Summary of the invention
[0005] The object of the present invention is to provide a grinding disc for uniform and efficient grinding of marble and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.
[0006] To achieve the above object, one of the objects of the present invention is to provide a grinding disc for uniformly grinding and efficiently opening marble, comprising the following raw materials in parts by weight:
[0007] 16.5-20.5 parts by weight of epoxy resin, 20-24 parts by weight of diamond, 6.5-8.5 parts by weight of resin curing agent, 12-16 parts by weight of mullite, 8-12 parts by weight of silicon carbide, 8-12 parts by weight of corundum, 11-15 parts by weight of wollastonite, and 4-6 parts by weight of pumice.
[0008] As a further improvement of the technical solution, the epoxy resin is an aminophenol trifunctional epoxy resin, and the resin curing agent is a diethyltoluenediamine epoxy resin curing agent.
[0009] As a further improvement of the present technical solution, the diamond is 50 mesh diamond particles, and the silicon carbide is 50 mesh silicon carbide.
[0010] The second object of the present invention is to provide a method for preparing the grinding disc for uniformly grinding marble as described above, comprising the following steps:
[0011] S1. First, epoxy resin and diamond are mixed to form a main material, and then the main material is put into a mixer for standby use;
[0012] S2, then put the resin curing agent, mullite, silicon carbide, corundum, wollastonite and pumice into the mixer in sequence and stir and mix with the main material;
[0013] S3, shaking and dispersing the above raw materials in a mixer to form a primary mixture, and evenly applying the primary mixture to a mold;
[0014] S4. The mold with the abrasive is placed in an oven for sufficient heating, so that after the primary mixture is cured, the abrasive disc with a specified shape is produced through demoulding and subjected to secondary curing.
[0015] As a further improvement of the technical solution, in S1, at room temperature of 15-25°C, 16.5-20.5 parts by weight of epoxy resin are added to a mixing barrel, and then 20-24 parts by weight of diamond are slowly added and preliminarily stirred evenly with a polytetrafluoroethylene stirring rod.
[0016] As a further improvement of the technical solution, in S2, at a humidity below 40%, 6.5-8.5 parts by weight of resin curing agent, 12-16 parts by weight of mullite, 8-12 parts by weight of silicon carbide, 8-12 parts by weight of corundum, 11-15 parts by weight of wollastonite, and 4-6 parts by weight of pumice are added respectively. After the powder is added, it is preliminarily stirred with a polytetrafluoroethylene stirring rod, and then put into a vibration mixer and mixed for 30-40 minutes.
[0017] As a further improvement of the technical solution, in S3, the materials are mixed evenly and then evenly applied to a mold with a diameter ranging from 80 to 100 mm and a thickness ranging from 2 to 4 mm.
[0018] As a further improvement of the technical solution, in S3, the scraping material is applied when the temperature of the abrasive tool is maintained at 15-25°C.
[0019] As a further improvement of the technical solution, in said S4, the heating temperature range for sufficient heating is 115-145°C, and the curing time range is 0.5-1.0h. Then demoulding, the product is placed in an oven and heated at 145°C for 2h. The product is taken out and the adhesive backing is cut and used.
[0020] As a further improvement of the technical solution, in S4, the roughness range of the output grinding disc is 50 mesh.
[0021] In the present invention, S1 is used to preliminarily mix epoxy resin, a material with the greatest viscosity, and diamond powder, a material with the greatest density, uniformly; S2 and S3 are used to uniformly mix other materials with the materials described in S1 to form abrasives with stable performance; and S4 is used to convert the uniformly mixed abrasives into abrasive discs and abrasive tools.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] In the grinding disc for uniform and efficient grinding of marble and the preparation method thereof, the epoxy resin with the greatest viscosity and the diamond powder with the greatest density are preliminarily mixed evenly, and then mixed evenly with other materials; the resin and the curing agent react under heating to form a polymer network structure; the inorganic filler and diamond powder added subsequently are uniformly wrapped to form a diamond grinding disc with stable performance; the grinding disc finally produced can uniformly and efficiently grind marble materials on the market and make them have better flatness. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is the overall flow chart of the present invention. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Abrasive discs are dry abrasive discs made by heating liquid resin and diamond material under specific conditions. Existing abrasive discs have low grinding efficiency and cumbersome procedures when grinding traditional hard stone materials such as granite, concrete, marble, quartz stone, etc., which greatly increases production and material costs. In the later stage, it also brings troubles such as high investment of time and financial resources and low returns to customers during use.
[0027] Therefore, one of the objects of the present invention is to provide a grinding sheet for uniformly grinding marble, comprising the following raw materials in parts by weight:
[0028] 16.5-20.5 parts by weight of epoxy resin, 20-24 parts by weight of diamond, 6.5-8.5 parts by weight of resin curing agent, 12-16 parts by weight of mullite, 8-12 parts by weight of silicon carbide, 8-12 parts by weight of corundum, 11-15 parts by weight of wollastonite, and 4-6 parts by weight of pumice;
[0029] Furthermore, the epoxy resin is aminophenol trifunctional epoxy resin, and the resin curing agent is diethyltoluenediamine epoxy resin curing agent. The resin and curing agent react under heating to form a polymer network structure to uniformly wrap the inorganic filler and diamond powder added subsequently to form a diamond grinding disc with stable performance. The selected epoxy resin and curing agent have the advantages of stable curing system and high curing efficiency.
[0030] Furthermore, the diamond is 50 mesh diamond particles, and the silicon carbide is 50 mesh silicon carbide. The scratches formed by the diamond and silicon carbide powders of different meshes when polishing the surface of the marble are uniform, stable and efficient, which is also conducive to coating and curing during the production process.
[0031] See also Figure 1 As shown, the second object of the present invention is to provide a method for preparing the grinding disc for uniformly grinding marble described above, and the specific steps are as follows:
[0032] S1. First, epoxy resin and diamond are mixed to form the main material, and then the main material is put into a mixer for standby use. At room temperature of 15-25°C, 16.5-20.5 parts by weight of epoxy resin are put into the mixing barrel, and then 20-24 parts by weight of diamond are slowly added and preliminarily stirred evenly with a polytetrafluoroethylene stirring rod. The temperature range when adding is 15-25°C.
[0033] S2. Then, the resin curing agent, mullite, silicon carbide, corundum, wollastonite and pumice are sequentially put into the mixer and stirred with the main material. When the humidity is below 40%, 6.5-8.5 parts by weight of the resin curing agent, 12-16 parts by weight of mullite, 8-12 parts by weight of silicon carbide, 8-12 parts by weight of corundum, 11-15 parts by weight of wollastonite and 4-6 parts by weight of pumice are added respectively. After the powder is added, it is preliminarily stirred with a polytetrafluoroethylene stirring rod, and then put into the oscillating mixer and mixed for 30-40 minutes.
[0034] S3, the raw materials are shaken and dispersed in a mixer to form a primary mixture, and the primary mixture is evenly applied to a mold, wherein the materials are mixed evenly and then evenly applied to a mold with a diameter range of 80-100 mm and a thickness range of 2-4 mm, and the mold temperature range during the even application is 15-25° C.;
[0035] S4. Fully heat the mold to make the initial mixture solidify, then demould to produce a grinding disc with a specified shape and solidify. The heating temperature range for full heating is 115-145℃, and the curing time range is 0.5-1.0h. Then demould, place the product in an oven at 145℃ for 2h, take out the product, cut the adhesive backing and use it. The roughness range of the produced grinding disc is 50 mesh, which is a stable and efficient marble grinding disc.
[0036] In the present invention, S1 is used to preliminarily mix the epoxy resin with the highest viscosity and the diamond powder with the highest density, S2 and S3 are used to mix other materials with the S1 material and form abrasives with stable performance, and S4 is used to convert the mixed abrasives into abrasive discs and abrasive tools.
[0037] According to the differences in the amount of raw materials and process parameters in the preparation process, the grinding disc for uniform and efficient grinding of marble prepared by the present invention is further described through the following specific examples.
[0038] Example 1
[0039] S1, first 18.5 parts by weight of epoxy resin and 22 parts by weight of diamond are mixed to form a main material, and then the main material is put into a mixer and reserved for standby;
[0040] S2, then 7.5 parts by weight of resin curing agent, 14 parts by weight of mullite, 10 parts by weight of silicon carbide, 10 parts by weight of corundum, 13 parts by weight of wollastonite, and 5 parts by weight of pumice are sequentially put into a mixer and stirred and mixed with the main material, the temperature when put in is 15 ° C, after the powder is put in, it is preliminarily stirred with a polytetrafluoroethylene stirring rod, and then put into a vibration mixer and mixed for 40 minutes;
[0041] S3, the raw materials are shaken and dispersed in a mixer to form a primary mixture, and the primary mixture is evenly applied to a mold, wherein the materials are mixed evenly and then evenly applied to a mold with a diameter of 80 mm and a thickness of 2 mm, and the mold temperature during the even application is 15°C;
[0042] S4. The mold is heated fully so that after the primary mixture is cured, the abrasive disc with a specified shape is produced through demoulding and dried. The heating temperature during the full heating is 130°C and the curing time is 1.0h. After the curing is completed, the mold is demoulded and the product is placed in an oven at 145°C for 2h. The product is taken out and cut to stick to the backing base. The roughness of the produced abrasive disc is 50 mesh.
[0043] Example 2
[0044] S1, first 18.5 parts by weight of epoxy resin and 22 parts by weight of diamond are mixed to form a main material, and then the main material is put into a mixer and reserved for standby;
[0045] S2, then 7.5 parts by weight of resin curing agent, 14 parts by weight of mullite, 10 parts by weight of silicon carbide, 10 parts by weight of corundum, 13 parts by weight of wollastonite, and 5 parts by weight of pumice are sequentially put into a mixer and stirred and mixed with the main material, the temperature when put in is 15 ° C, after the powder is put in, it is preliminarily stirred with a polytetrafluoroethylene stirring rod, and then put into a vibration mixer and mixed for 40 minutes;
[0046] S3, the raw materials are shaken and dispersed in a mixer to form a primary mixture, and the primary mixture is evenly applied to a mold, wherein the materials are mixed evenly and then evenly applied to a mold with a diameter of 100 mm and a thickness of 2 mm, and the mold temperature during the even application is 15°C;
[0047] S4. The mold is heated fully so that after the primary mixture is cured, the abrasive disc with a specified shape is produced through demoulding and dried. The heating temperature during the full heating is 130°C and the curing time is 1.0h. After the curing is completed, the mold is demoulded and the product is placed in an oven at 145°C for 2h. The product is taken out and cut to stick to the backing base. The roughness of the produced abrasive disc is 50 mesh.
[0048] Example 3
[0049] S1. First, 16.5 parts by weight of epoxy resin and 24 parts by weight of diamond are mixed to form a main material, and then the main material is put into a mixer and set aside;
[0050] S2, then 6 parts by weight of resin curing agent, 11.5 parts by weight of mullite, 10 parts by weight of silicon carbide, 10 parts by weight of corundum, 15 parts by weight of wollastonite, and 7 parts by weight of pumice are sequentially put into a mixer and stirred and mixed with the main material, the temperature when put in is 20°C, after the powder is put in, it is preliminarily stirred with a polytetrafluoroethylene stirring rod, and then put into a shaking mixer and mixed for 35 minutes;
[0051] S3, the raw materials are shaken and dispersed in a mixer to form a primary mixture, and the primary mixture is evenly applied to a mold, wherein the materials are mixed evenly and then evenly applied to a mold with a diameter of 100 mm and a thickness of 2 mm, and the mold temperature during the even application is 20°C;
[0052] S4. The mold is fully heated so that after the primary mixture is cured, the abrasive disc with a specified shape is produced through demoulding and dried. The heating temperature during full heating is 135°C and the curing time is 0.9h. After curing, the product is demoulded and placed in an oven at 145°C for 2h. The product is taken out and cut to stick to the backing. The roughness of the produced abrasive disc is 50 mesh.
[0053] Example 4
[0054] S1, first 20.5 parts by weight of epoxy resin and 20 parts by weight of diamond are mixed to form a main material, and then the main material is put into a mixer and reserved for standby;
[0055] S2, then 8.3 parts by weight of resin curing agent, 13 parts by weight of mullite, 9 parts by weight of silicon carbide, 11 parts by weight of corundum, 12.2 parts by weight of wollastonite, and 6 parts by weight of pumice are sequentially put into a mixer and stirred and mixed with the main material, the temperature when put in is 25°C, after the powder is put in, it is preliminarily stirred with a polytetrafluoroethylene stirring rod, and then put into a shaking mixer and mixed for 30 minutes;
[0056] S3, the above raw materials are shaken and dispersed in a mixer to form a primary mixture, and the primary mixture is evenly applied to a mold, wherein the materials are mixed evenly and then evenly applied to a mold with a diameter of 100 mm and a thickness of 4 mm, and the mold temperature during the even application is 25°C;
[0057] S4. The mold is heated fully so that after the primary mixture is cured, the abrasive disc with a specified shape is produced through demoulding and dried. The heating temperature during the full heating is 140°C and the curing time is 0.8h. After the curing is completed, the mold is demoulded and the product is placed in an oven and heated at 145°C for 2h. The product is taken out and cut to stick to the backing base. The roughness of the produced abrasive disc is 50 mesh.
[0058] Table 1 Comparison of the difference in raw material dosage in Examples 1-4
[0059]
[0060] Table 2 Comparison of process parameters in Examples 1-4
[0061]
[0062] Comparative Example 1
[0063] This comparative example adopts the preparation method of Example 1, except that the diamond roughness is changed to 60, and the rest remains unchanged. The specific steps are similar to those of Example 1, and will not be repeated in this comparative example.
[0064] Comparative Example 2
[0065] This comparative example adopts the preparation method of Example 1, except that the diamond roughness is changed to 120, and the rest remains unchanged. The specific steps are similar to those of Example 1, and will not be repeated in this comparative example.
[0066] Table 3 Comparison of process parameters between Example 1 and Comparative Examples 1-2
[0067]
[0068] Comparative Example 3
[0069] This comparative example adopts the preparation method of Example 3, and the heating temperature is set to 150° C., and the rest remains unchanged. The specific steps are similar to those of Example 2, and will not be repeated in this comparative example.
[0070] Comparative Example 4
[0071] This comparative example adopts the preparation method of Example 3, and sets the curing time to 1.5 h, while the rest remain unchanged. The specific steps are similar to those of Example 2, and will not be described in detail in this comparative example.
[0072] Comparative Example 5
[0073] This comparative example adopts the preparation method of Example 3, and the roughness is set to 40 meshes, and the rest remains unchanged. The specific steps are similar to those of Example 2, and will not be repeated in this comparative example.
[0074] Table 4 Comparison of process parameters in Example 3 and Comparative Examples 3-5
[0075]
[0076] Comparative Example 6
[0077] This comparative example adopts the preparation method of Example 4, the input temperature is set to 0°C, and the rest remains unchanged. The specific steps are similar to those of Example 3, and will not be repeated in this comparative example.
[0078] Comparative Example 7
[0079] This comparative example adopts the preparation method of Example 4, and the mixing time is set to 20 minutes, and the rest remains unchanged. The specific steps are similar to those of Example 3, and will not be repeated in this comparative example.
[0080] Comparative Example 8
[0081] This comparative example adopts the preparation method of Example 4, and the mold temperature is set to 100° C., and the rest remains unchanged. The specific steps are similar to those of Example 3, and will not be repeated in this comparative example.
[0082] Table 5 Comparison of process parameters in Example 4 and Comparative Examples 6-8
[0083]
[0084] Test example
[0085] Grinding discs were prepared according to the preparation methods provided in Examples 1-4 and Comparative Examples 1-8, and the prepared grinding discs were bonded to an angle grinder to evenly grind the black and white marble. The grinding amount per minute was recorded, and the average grinding amount was recorded in Table 6.
[0086] Table 6 Comparison of grinding amount of the grinding discs of the embodiment and the comparative example
[0087] Average grinding amount per minute / g Example 1 8.9 Example 2 11.2 Example 3 10.3 Example 4 10.5 Comparative Example 1 6.3 Comparative Example 2 1.7 Comparative Example 3 / (High curing temperature makes demoulding impossible) Comparative Example 4 / (Long curing time and unable to demould) Comparative Example 5 / (The diamond particles are large, the abrasive tool is seriously damaged, and the marble surface is scratched) Comparative Example 6 / (Unable to mix evenly) Comparative Example 7 / (Mixing time is insufficient, mixing is uneven, and grinding performance is unstable) Comparative Example 8 / (The mold temperature is high, which prolongs the entire curing time and makes demoulding impossible)
[0088] According to Table 6, compared with Examples 1-8, the grinding amount of the grinding discs prepared in Examples 1-4 is greater than that of the grinding discs prepared in the comparative examples, and the grinding amount of the grinding discs prepared in the Examples is stable and the scratches are uniform, while the grinding amount of the grinding discs prepared in the comparative examples with different raw material amounts and process parameters is reduced or the grinding discs cannot be prepared normally. Therefore, under the working conditions of this embodiment, the grinding efficiency of the prepared grinding discs is better.
[0089] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing a grinding disc for uniform and efficient grinding of marble, It is characterized in that The following steps are involved: S1. First, 16.5-20.5 parts by weight of epoxy resin and 20-24 parts by weight of diamond are mixed to form a main material, and then the main material is put into a mixer and set aside; S2, then 6.5-8.5 parts by weight of a resin curing agent, 12-16 parts by weight of mullite, 8-12 parts by weight of silicon carbide, 8-12 parts by weight of corundum, 11-15 parts by weight of wollastonite, and 4-6 parts by weight of pumice are sequentially put into a mixer and stirred and mixed with the main material; S3, shaking and dispersing the above raw materials in a mixer to form a primary mixture, and evenly applying the primary mixture to a mold; S4. The mold with the abrasive is placed in an oven for sufficient heating, so that after the primary mixture is cured, the abrasive disc with a specified shape is produced through demoulding and subjected to secondary curing.
2. The method for preparing a grinding disc for uniformly grinding marble according to claim 1, Features: In the S1, the epoxy resin is aminophenol trifunctional epoxy resin, and the diamond is 50 mesh diamond particles.
3. The method for preparing a grinding disc for uniformly grinding marble according to claim 1, Features: In S1, epoxy resin is first put into a mixing barrel, and then diamond is slowly put into the mixing barrel and preliminarily stirred evenly with a polytetrafluoroethylene stirring rod, and the temperature range of the putting in the mixing barrel is 15-25°C.
4. The method for preparing a grinding disc for uniformly grinding marble according to claim 1, Features: In S2, the resin curing agent is diethyltoluenediamine epoxy resin curing agent, and the silicon carbide is 50 mesh silicon carbide.
5. The method for preparing a grinding disc for uniformly grinding marble according to claim 1, Features: In S2, when the humidity is below 40%, resin curing agent, mullite, silicon carbide, corundum, wollastonite and pumice are added respectively, and the powder is initially stirred with a polytetrafluoroethylene stirring rod, and then put into a vibration mixer for mixing, and the mixing time range is 30-40 minutes.
6. The method for preparing a grinding disc for uniformly grinding marble according to claim 1, Features: In S3, the materials are mixed evenly and then evenly applied to a mold, the diameter of the mold is in the range of 80-100 mm and the thickness is in the range of 2-4 mm.
7. The method for preparing a grinding disc for uniformly grinding marble according to claim 6, Features: The mold temperature range for uniform coating is 15-25°C.
8. The method for preparing a grinding disc for uniformly grinding marble according to claim 1, Features: In the S4, the heating temperature range for sufficient heating is 115-145°C, and the curing time range is 0.5-1.0h. After the curing is completed, demoulding is performed, and the product is placed in an oven and heated at 145°C for 2h, and the product is taken out and the adhesive backing is cut.
9. The method for preparing a grinding disc for uniformly grinding marble according to claim 1, Features: In the S4, the roughness range of the produced grinding disc is 50 mesh.
10. A grinding disc for uniform and efficient grinding of marble prepared according to the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Epoxy resin type diamond grinding pad and manufacturing method thereof
CN103465155A
Preparation method of superhard resin grinding wheel
CN107775548A
grinding wheel manufacturing process
FR1312449A
Ceramic-bonded abrasive grinding tools
US5366524A