Preparation method of large-size high-purity alpha-Fe16N2 iron nitride magnetic powder

Through high-pressure roll mill and nano-sand mill coordinating activation of iron concentrate, controlling hydrogen reduction and nitriding conditions, the problem of difficult to prepare high-purity, micron-scale particle size α″-Fe16N2 iron nitride powder in the prior art is solved, and high-quality iron nitride powder is achieved The preparation of performance magnetic powder is suitable for magnet applications in high-tech industries.

CN118954444AActive Publication Date: 2024-11-15CENT SOUTH UNIV

Patent Information

Application Number
CN202411452888.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-17
Publication Date
2024-11-15
Estimated Expiration
2044-10-17

AI Technical Summary

Technical Problem

It is difficult to prepare high-purity, micron-scale large-size α″-Fe16N2 ferromagnetic nitride powder, and its stability is poor at high temperatures, making it difficult to meet the needs of high-performance magnets.

Method used

The iron concentrate is activated by high-pressure roller mill and nano-sand mill to control the hydrogen reduction temperature and nitriding conditions. The surface properties of the iron concentrate are changed through high-pressure roller mill. The nano-sand mill imparts mechanical energy storage to form porous active iron particles and achieve low temperatures. Nitriding reaction prepared a high-purity, large-size α″-Fe16N2 ferromagnetic nitride powder.

Benefits of technology

A large-size α″-Fe16N2 ferromagnetic powder with high purity and micron-sized particle size has been obtained, with excellent magnetic properties, suitable for alternative rare earth permanent magnets, and is suitable for high-performance magnet applications such as electric vehicles and wind power facilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954444A_ABST
    Figure CN118954444A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of large-size high-purity alpha ''-Fe16N2 iron nitride magnetic powder, which comprises the following steps: 1) sequentially carrying out high-pressure roller milling, nanometer sand milling and drying treatment on iron ore concentrate to obtain micron-sized fine-particle iron oxide powder; 2) performing hydrogen reduction on the micron-sized fine-particle iron oxide powder to obtain porous active reduced iron powder; the temperature of hydrogen reduction is controlled to be 50 DEG C lower than the critical temperature of a reduction conversion path; and 3) nitriding the porous active reduced iron powder in an ammonia atmosphere to obtain alpha-Fe16N2 iron nitride, the method takes cheap iron ore concentrate as a raw material, is low in cost and simple in process, can be used for mass production, can obtain micron-sized high-purity alpha-Fe16N2 iron nitride powder, and further can be molded by adopting a conventional additive manufacturing method to produce high-performance magnets.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an α"-Fe 16 Preparation method of N2 iron nitride magnetic powder, particularly a method for preparing large-size α"-Fe by synergistic activation of high-pressure roller mill and nano sand mill 16 The invention relates to a method for N2 nitriding iron powder, and belongs to the technical field of magnetic powder material preparation. Background Art

[0002] Permanent magnetic materials are widely used. The current high-quality permanent magnetic materials are made of rare earth permanent magnets represented by Nd-Fe-B. They have high coercive force, but the maximum magnetic energy product (BH) max is limited by the low Ms value of the rare earth compounds themselves, and cannot achieve greater breakthroughs. This is especially limited in their application in high-tech industries such as electric vehicles and wind power generation facilities. In addition, the rare earth metal elements required for rare earth permanent magnets are expensive and face the risk of resource depletion, and their mining volume is difficult to meet the needs of the rapidly developing new energy field. Therefore, the development of new zero-rare earth high-performance permanent magnetic materials is undoubtedly an important guarantee for solving future energy problems. At present, iron nitride is the most likely type of material to replace rare earth permanent magnets on a large scale. Iron nitride includes a variety of compounds such as FeN, Fe2N, Fe3N, Fe4N, among which α″-Fe 16 N2 compounds are the materials with the highest saturation magnetic induction intensity discovered so far, and have characteristics such as relatively high magnetocrystalline anisotropy, which almost meet all the requirements of high-performance magnets for material properties. α″-Fe 16 N2 is composed of Fe and N elements, with abundant reserves and low price, but it has poor stability at high temperatures and is easily decomposed above 200°C. The current preparation method using methods such as magnetron sputtering has great limitations in terms of output, purity and cost. The difficulty in the reduction nitridation method lies mainly in how to achieve nitridation of iron in an extremely low temperature range below the decomposition temperature.

[0003] In the prior art, the nitriding process is mainly promoted by refining the iron powder particle size, and is assisted by strengthening means such as reaction pressure or external field. For example, a Chinese patent (publication number: CN105861978A) discloses a mechanical ball milling preparation method for nitrided iron magnetic powder. ) discloses Fe as a permanent magnet 16 The preparation method of N2 compound, the Chinese patent (publication number: CN106086776A) discloses a low temperature plasma nitridation preparation method of nitrided iron magnetic powder, etc. In general, the α″-Fe 16N2 materials are mostly ultra-thin coatings or nano-sized particles, which are not suitable for forming high-performance magnets by pressing or bonding, especially when preparing large particle products, their purity cannot be guaranteed. Therefore, the existing α″-Fe 16 N2 material urgently needs to be improved in purity and particle size. Summary of the invention

[0004] It is difficult to prepare high-purity α"-Fe with micron-sized particles in the existing technology. 16 N2 and other technical problems, the purpose of the present invention is to provide a micron-sized, high-purity α"-Fe 16 The invention discloses a method for preparing N2 ferrous nitride magnetic powder.

[0005] The large-size high-purity α″-Fe 16 N2 iron nitride magnetic powder, wherein "large size" refers to micron-level particle size, preferably 5-40 μm, more preferably 10-30 μm. "High purity" refers to a pure phase iron nitride mass content of more than 97%, preferably more than 98%.

[0006] In order to achieve the above technical objectives, the present invention provides a large-sized high-purity α"-Fe 16 The method for preparing N2 iron nitride magnetic powder comprises the following steps:

[0007] 1) The iron ore concentrate is sequentially subjected to high-pressure roller milling, nano-sand milling and drying treatment to obtain micron-sized fine-particle iron oxide powder; the conditions of the high-pressure roller mill are as follows: the feed particle size of the iron ore concentrate is 40-100µm, the roller spacing is 100-150µm, the roller pressure is 10-20MPa, and the number of high-pressure roller cycles is 1-5 times; the conditions of the nano-sand milling are as follows: the diameter of the grinding beads is 0.05mm-0.5mm, the grinding speed is not less than 2000r / min, the grinding time is not more than 30min, the grinding medium is water, and the solid-liquid mass volume ratio is 1g:0.5-3mL; the conditions of the drying treatment are as follows: vacuum drying is adopted, the air pressure is 90-100KPa, and the temperature is 60-100°C;

[0008] 2) hydrogen reduction of micron-sized fine-particle iron oxide powder to obtain porous active reduced iron powder; the temperature of the hydrogen reduction is controlled to be within 50°C below the critical temperature of the reduction conversion path, wherein the critical temperature of the reduction conversion path refers to the temperature at the intersection of the iron oxide hydrogen reduction fork curve;

[0009] 3) The porous active reduced iron powder is nitrided in an ammonia atmosphere to obtain α″-Fe 16 N2 Iron Nitride.

[0010] The technical solution of the present invention can obtain large-sized high-purity α"-Fe 16The key to N2 nitrided iron magnetic powder is to obtain micron-sized iron particles with porous structure, high specific area and high activity by controlling the reduction process of iron concentrate. The iron particles with this structure are more conducive to low-temperature nitriding process and nitriding reaction, thereby obtaining high-purity and large-sized α″-Fe 16 N2 nitride iron magnetic powder. More specifically, the technical solution of the present invention first uses the technical means of high-pressure roller milling and nano-sand milling to coordinate mechanical activation of iron concentrate to prepare high-activity micron-level iron oxide powder, wherein the high-pressure roller milling process hardly changes the particle size of the iron concentrate, mainly causing cracks on the surface of the iron concentrate, reducing its mechanical strength and increasing its reaction activity, and its activation mechanism for the iron concentrate mainly comes from the extrusion and shearing effect under high pressure between the rollers, which can change the surface properties of the iron concentrate, while the nano-sand milling is to achieve its activation by impacting and grinding the iron concentrate on the high-speed rotating grinding disc through the medium, and the nano-sand milling process has a more obvious change in the particle size of the iron concentrate, so the activation mechanism of the nano-sand milling and the high-pressure roller milling is opposite and complementary, and the present invention combines the two technical means of high-pressure roller milling and nano-sand milling to activate the iron concentrate, which can give it great activation energy storage and can ensure that the iron concentrate has a micron-level particle size. On this basis, by strictly controlling the hydrogen reduction temperature, the hydrogen reduction process conversion path is controlled to be Fe3O4→Fe, so that porous active reduced iron powder can be obtained, which is beneficial to improve the reaction activity and rate of the low-temperature nitriding process, and then the micron-sized, high-purity α″-Fe 16 N2 Iron Nitride.

[0011] As a preferred solution, the iron concentrate has a total iron content of more than 71.5%. The iron concentrate is a pure iron concentrate, mainly including deep ore dressing concentrate and iron phosphorus, iron slag, etc. in the metallurgical processing process, characterized by a total iron content of more than 71.5%, and the remaining impurities are silicon, manganese, aluminum and other substances and their oxides. According to the ore dressing means in the prior art, iron concentrate with a total iron content of more than 71.5% is easy to obtain and belongs to a relatively cheap iron raw material.

[0012] The high pressure roller mill of the present invention has a wide adaptability to the particle size of iron concentrate raw materials, and can be directly used for iron concentrate with a particle size of 40-100 μm in beneficiation or primary processing. The roller spacing is mainly selected and set according to the feed particle size of the iron concentrate. The key to the high pressure roller mill process is the setting of the roller pressure. The roller pressure has a significant effect on the grinding activation effect. The further preferred roller pressure range is 15-20 MPa. Since the high pressure roller mill has the defect of large edge effect, the iron concentrate is set to 2-4 grinding cycles to achieve a better roller pressure level.

[0013] The nano-sand mill of the present invention can give the iron concentrate rich mechanical energy storage and active sites, and the further preferred bead diameter range is 0.05~0.2mm. The further preferred grinding speed range is 2500~3000r / min. Based on the low strength of the iron concentrate after high-pressure roller milling, it is easy to cause over-grinding under the high-speed grinding action of the nano-sand milling, so it is necessary to control the activation within a very short grinding time, and the grinding time is controlled within 30min, which will not cause excessive refinement of the particles, and the further preferred grinding time is 10~20min. In addition, since the high-pressure roller milling changes the hydrophilicity of the surface of the iron concentrate particles, water can be selected as the medium during the nano-sand milling process, and there is no need to add grinding aids, dispersion and other additives, and the introduction of new impurities can be avoided as much as possible. The present invention grinds large-particle materials with mismatched small grinding beads and activates the materials in combination with roller milling, so that the iron concentrate can be activated in a short time, and the micron-level particle size characteristics are retained.

[0014] The drying and dehydration of the present invention is to reduce the water content of the iron ore concentrate, which is beneficial to the subsequent hydrogenation process. Low-temperature vacuum drying is beneficial to preventing the agglomeration of particles, and the material dried by this drying method often presents a porous loose structure, which is beneficial to the subsequent gas-solid reaction. If the iron ore concentrate material has agglomeration after drying, it can be broken up by conventional means, such as ultrasound, grinding, etc.

[0015] As a preferred solution, the particle size of the micron-sized fine iron oxide powder is 10-30µm, and the activated lattice size is 150-800Å. Under the synergistic activation of the high-pressure roller mill and the nano-sand mill, the particle size of the iron concentrate is not greatly refined, but the mechanical activation effect is more prominent. The activated lattice size is refined to 150-800Å in the XRD detection characteristics, indicating that the reaction activity of the iron concentrate is greatly improved, which is beneficial to the subsequent hydrogen reduction process.

[0016] As a preferred solution, the conditions for hydrogen reduction are: the temperature is 20~50℃ lower than the critical temperature of the reduction conversion path, and the time is 2~5h. Generally speaking, in the process of preparing iron powder by hydrogen reduction of iron ore, in order to ensure the reduction efficiency of iron ore, the hydrogen reduction temperature is controlled to be higher than the critical temperature of the reduction conversion path. The key to the technical solution of the present invention is to control the hydrogen reduction temperature within the range of 20~50℃ lower than the critical temperature of the reduction conversion path. For example, the critical temperature of the reduction conversion path of a certain micron-sized iron ore is 500℃, and the technical solution of the present invention controls the hydrogen reduction temperature below the critical temperature of the reduction path conversion (preferably reduced at 450~480℃), so that the reduction path follows the Fe3O4→Fe reduction path, rather than the Fe3O4→FeO→Fe reduction path. The Fe3O4→Fe reduction path can make the iron ore particles expand during the reduction process, and the particle size increases. After reduction, the iron ore particles are 12~35µm, and the particles show an embedded porous structure, with developed voids deep inside the particles, and their specific surface area is not less than 10m 2 / g, the preferred specific surface area range is 20~30 m 2 / g. However, the reduction temperature cannot be too low, otherwise it will be difficult to completely reduce the iron oxide within a suitable time. During the hydrogen reduction process, micron-sized fine iron oxide powder is loosely distributed on the reactor, and the general material layer thickness is 1~5mm.

[0017] As a preferred solution, the critical temperature of the reduction path conversion of the micron-sized fine-particle iron oxide powder relative to the iron concentrate is reduced to 350~520°C based on the activation effect of the high-pressure roller mill and the nano-sand mill. The method for determining the critical temperature of the reduction path conversion of the present invention is: 1) Theoretical calculation method, based on the mechanical activation theory and XRD detection, calculates the size of the mechanical energy storage during the activation process, and the temperature point compared with the curve after the iron oxide energy storage is calculated in combination with the Gibbs free energy is the critical temperature. 2) Experimental detection method, testing the composition of the material phase of the reduction process at different reduction temperatures, the temperature point where the FeO phase does not appear below a certain temperature is the critical temperature. According to the actual grinding energy storage situation, this temperature point is between 350~520°C, which is about 20~220°C lower than the critical temperature point of 570°C for the reduction path conversion of conventional iron concentrate.

[0018] As a preferred solution, the nitriding conditions are: ammonia pressure is not higher than 0.5MPa, nitriding temperature is 170-195°C, and time is 8-15h. Based on the micron-sized iron particles with porous structure, high specific area and high activity, the nitriding process becomes easier to produce α″-Fe 16 The purity of N2 iron nitride is above 97%, preferably above 98%. The ammonia atmosphere is more preferably a pure ammonia atmosphere.

[0019] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects:

[0020] 1) α″-Fe prepared by the present invention 16 N2 iron nitride magnetic powder is the material with the greatest potential to replace rare earth permanent magnets on a large scale. Compared with existing rare earth permanent magnets, the product has the advantages of abundant raw material reserves, low price, sufficient supply, large-scale preparation, and green production process, without worrying about the quota supply of rare earth elements and resource depletion.

[0021] 2) The present invention prepares pure phase and highly amorphous α″-Fe 16 N2 iron nitride magnetic powder has higher coercive force than similar products, and has the "giant magnetic moment" phenomenon, with the best saturation magnetization intensity. The improved comprehensive magnetic properties are likely to be better than rare earth permanent magnet materials, and are suitable for fields such as electric vehicles and wind power generation facilities that have higher requirements for magnet performance.

[0022] 3) The present invention prepares pure phase α″-Fe on a larger (micrometer) scale 16 N2 magnetic powder particles have reached the processing and forming particle size range of rare earth magnetic powder with existing technology. Compared with the currently prepared microscopic iron nitride, it is more suitable for magnetic powder pressing and bonding and other material processing, and has higher practical value. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a thermodynamic calculation diagram of the mechanical energy storage of the 6-15µm iron concentrate obtained by high pressure roller milling and nano sand milling in Example 1. It can be seen from the figure that due to the existence of activated energy storage, the conversion temperature of the reduction path is converted from 571°C to 465°C.

[0024] Figure 2 This is the apparent image of the micron-sized iron concentrate obtained by high-pressure roller milling and nano-sand milling after hydrogen reduction in Example 1; it can be seen from the figure that the iron powder presents a porous structure, which is extremely beneficial to the gas permeation in the subsequent solid-gas reaction process.

[0025] Figure 3 The α″-Fe prepared in Example 1 16 XRD diagram of N2 material; the figure shows α″-Fe 16 N2 is a pure phase product with almost no other impurities, indicating a high degree of nitridation.

[0026] Figure 4 This is a scanning electron microscope image of the iron powder prepared in Control Example 1; as can be seen from the image, the surface of the iron powder is sintered, with a high degree of density and low reaction activity, which is not conducive to the subsequent solid-gas reaction process.

[0027] Figure 5 α″-Fe prepared in Comparative Example 1 16XRD diagram of N2 material; it can be seen from the figure that due to the insufficient activity of iron powder, the nitridation reaction is still not sufficient after a long period of nitridation, and the material is mainly Fe phase.

[0028] Figure 6 α″-Fe prepared in Comparative Example 2 16 XRD diagram of N2 material; it can be seen from the figure that α″-Fe 16 The purity of N2 is not high, which means that the activation degree of a single activation method is not high, and the purity of the prepared product is lower at the same level. DETAILED DESCRIPTION

[0029] In order to more clearly understand the present invention, specific embodiments are now used to more clearly explain and analyze the contents of the present invention. However, the claims of the present invention are not limited to the following example methods and conditions. Other examples obtained by relevant technical personnel in the field without creative work are all within the protection scope of the present invention.

[0030] Example 1

[0031] The raw material is high-quality iron scale from a steel rolling mill. The purity is 72.1% iron, and the total content of other impurities (acid insolubles) is only 0.3%. The main components are high-purity iron oxides, which are different from iron concentrates in that there are more Fe2O 3, After the test, more than 96% of the particle size after beneficiation is between -200 mesh (200 mesh sieve) and +325 mesh (325 mesh sieve). Set the high-pressure roller mill, the roller spacing is 150µm, the roller pressure is 12MPa, set the appropriate feed rate, and cycle grinding for 5 times. After testing, the particle size D 50 The material was finely ground in a nano sand mill. A high-efficiency pin-type nano sand mill was selected with a rotation speed of 2000 r / min, a 0.1 mm zirconia ball, water as solvent, and a solid-liquid ratio of 1 g: 3 mL. After grinding for 10 min, a particle size D 50 =30µm ultrafine particle slurry was dried at low temperature vacuum (95KPa, 80℃) for 3 hours to obtain powder.

[0032] The powder lattice size was found to be about 420Å by testing the powder lattice characteristics and other properties. The changes in the hydrogen reduction thermodynamic diagram after activation were calculated by combining the mechanical activation energy and other key parameters. Figure 1 As shown in Figure 2, the critical temperature of the reduction conversion path is about 465°C.

[0033] The reduction temperature of the powder reduction stage was controlled to be 430℃. The agglomerates were loosely spread on the reduction steel belt with a height of 2mm. Pure hydrogen was used as the reduction gas for 3h. After the reduction, the iron powder had slight agglomeration. After subsequent breaking up, the purity of the iron powder was 99%. The powder was placed in a tubular reactor, and pure ammonia was introduced to control the pressure at about 0.2MPa. The pure phase sample was obtained by nitridation at 175℃ for 15h. After XRD quantitative calculation, the obtained pure phase α″-Fe 16 The purity of N2 magnetic powder is 98.6%.

[0034] Example 2

[0035] The super iron concentrate obtained by deep beneficiation is selected as raw material, with an iron grade of 72.1% and the total content of other impurities (acid insoluble matter) is only 0.3%. The particle size of the material after deep beneficiation is small. After testing, more than 96% of the particle size after beneficiation is between -200 mesh and +325 mesh. Set a high-pressure roller mill with a roller spacing of 100µm and a roller pressure of 18MPa. Set an appropriate feed rate, grind once, and test the particle size D after grinding. 50 The material is then finely ground in a nano sand mill. A high-efficiency pin-type nano sand mill is selected with a rotation speed of 2500r / min, 0.05mm zirconia balls as grinding beads, water as solvent, and a solid-liquid ratio of 1g:0.5mL. After grinding for half an hour, an ultrafine particle slurry with a particle size of D50=20µm is obtained, which is then dried at a vacuum low temperature (93KPa, 70°C) for 5 hours to obtain a powder.

[0036] By testing the powder lattice characteristics and other properties, the powder lattice size was measured to be 154Å. Combined with other lattice parameters, the lattice energy storage was calculated through mechanical activation theory and supported by experimental data, the critical temperature of the reduction transformation path is about 350℃.

[0037] In the powder reduction stage, the reduction temperature was controlled at 300 °C. The agglomerates were loosely spread on the reduction steel belt with a spreading height of 1 mm. Pure hydrogen was used as the reducing gas for 5 h. After the reduction, the iron powder had slight agglomeration. After subsequent breaking up, the purity of the iron powder was tested to be 99.15%, and the particle size was about 25 µm. The morphology of the iron powder is shown in the figure. Figure 2 The powder was also placed in a belt reactor with a thickness of 3 mm. The reaction temperature was controlled at 195 °C and nitrided under pure ammonia at normal pressure for 8 h to obtain a pure phase sample. The XRD pattern of the sample was as follows: Figure 3 As shown, there are almost no other impurities. After XRD quantitative calculation, the pure phase α″-Fe 16 The purity of N2 magnetic powder is 99.2%.

[0038] Example 3

[0039] The same super iron concentrate as in Example 2 was selected as the raw material. The raw material was first subjected to high-pressure roller milling, with a roller spacing of 130 μm and a roller pressure of 20 MPa, and a suitable feed rate was set for grinding 3 times, and then the material was finely ground in a nano sand mill, and a high-efficiency pin-type nano sand mill was selected, with a rotation speed of 3000 r / min, a grinding bead of 0.2 mm zirconium oxide ball, water as solvent, and a solid-liquid ratio of 1 g: 1 mL. After grinding for 15 min, an ultrafine particle slurry with a particle size of D50 = 22 μm was obtained, which was dried at a vacuum low temperature (93 KPa, 100 ° C) for 2 hours to obtain a powder.

[0040] By testing the powder lattice characteristics and other properties, the powder lattice size was measured to be 621Å. Combined with other lattice parameters, the lattice energy storage was calculated through mechanical activation theory and supported by experimental data. After activation, the temperature of the fork curve intersection of its hydrogen reduction thermodynamic diagram was 495℃.

[0041] During the powder reduction stage, the reduction temperature was controlled at 450°C. The agglomerates were loosely spread on the reduction steel belt with a spread height of 3mm. Pure hydrogen was used as the reduction gas and the reduction was carried out for 3 hours. After the reduction, the iron powder had slightly agglomerated. After subsequent breaking up, the iron powder purity was tested to be 98.85% and the particle size was about 25µm. The powder was also arranged in a belt reactor with a spread thickness of 2mm. The reaction temperature was controlled at 195°C and nitrided under pure ammonia at normal pressure for 11 hours to obtain a pure phase sample. There were almost no other impurities in the sample test. After XRD quantitative calculation, the obtained pure phase α″-Fe 16 The purity of N2 magnetic powder is 98.4%.

[0042] Example 4

[0043] The same super iron concentrate as in Example 2 was selected as the raw material. The raw material was first subjected to high-pressure roller milling, with a roller spacing of 130 μm and a roller pressure of 15 MPa. The appropriate feed rate was set and the material was ground 4 times. Then the material was finely ground in a nano sand mill. A high-efficiency pin-type nano sand mill was selected with a rotation speed of 2700 r / min, a grinding bead of 0.5 mm zirconium oxide ball, water as solvent, and a solid-liquid ratio of 1 g: 2 mL. After grinding for 30 min, an ultrafine particle slurry with a particle size of D50 = 27 μm was obtained, which was dried at a vacuum low temperature (93 KPa, 100 ° C) for 2 hours to obtain a powder.

[0044] By testing the powder lattice characteristics and other properties, the powder lattice size was measured to be 800Å. Combined with other lattice parameters, the lattice energy storage was calculated through mechanical activation theory and supported by experimental data. After activation, the temperature of the fork curve intersection of its hydrogen reduction thermodynamic diagram was 520℃.

[0045] During the powder reduction stage, the reduction temperature was controlled at 500°C. The agglomerates were loosely spread on the reduction steel belt with a spreading height of 5mm. After reduction for 5 hours, the iron powder had slightly agglomerated. After subsequent breaking up, the purity of the iron powder was 98.65% and the particle size was about 30µm. The powder was also arranged in a belt reactor with a spreading thickness of 1mm. The reaction temperature was controlled at 195°C. Ammonia was introduced to control the pressure at 0.5MPa. A pure phase sample was obtained by nitriding under pure ammonia at normal pressure for 13 hours. There were almost no other impurities in the sample test. After XRD quantitative calculation, the obtained pure phase α″-Fe 16 The purity of N2 magnetic powder is 97.8%.

[0046] Comparative Example 1

[0047] This control example is mainly used to illustrate the difference between controlling the hydrogen reduction temperature within and outside the critical temperature range of the hydrogen reduction path conversion.

[0048] Compared with Example 1, the only difference is that the hydrogen reduction temperature is set to 500°C, which is higher than the critical temperature of the reduction conversion path, and is not lower than the critical temperature of the reduction conversion path within the range of 20 to 50°C as required. The morphology image of the iron powder after hydrogen reduction is as follows: Figure 4 As shown in the figure, the iron powder surface has no deep pores, which will limit the ammonia permeation reaction. The iron powder is nitrided under the same conditions as in Example 1 to obtain α″-Fe 16 N2 sample, α″-Fe 16 The XRD pattern of N2 sample is shown in Figure 5 As shown, the product purity is low.

[0049] Comparative Example 2

[0050] This comparative example is mainly used to illustrate that it is difficult to fully activate iron concentrate by using a single high pressure roller mill or nano-grinding.

[0051] Compared with Example 1, the only difference is that only high-pressure roller mill is used, and the roller mill material is not subjected to nano-sand grinding, but directly subjected to hydrogen reduction. The results show that the activation purity of a single high-pressure roller mill is insufficient, and it can only be quickly reduced at a temperature above 700°C. The obtained iron powder is agglomerated and has a small specific surface area, making it difficult to complete the subsequent nitridation process.

[0052] Comparative Example 3

[0053] This comparative example is mainly used to illustrate that it is difficult to fully activate iron concentrate by using a single high pressure roller mill or nano-grinding.

[0054] Compared with Example 1, the only difference is that only nano-sand milling is used, and the iron ore concentrate is not subjected to high-pressure roller milling. After nano-sand milling, hydrogen reduction is performed. The results show that the activation degree of single impact and grinding is also insufficient. Without the cooperation of high-pressure roller milling, the same grinding conditions can achieve a critical temperature of about 480°C, and the particle cracks and other activation features are less. The XRD image of the product prepared after reduction and nitridation under the same conditions is as follows: Figure 6 shown.

[0055] Comparative Example 4

[0056] Compared with Example 1, the only difference is that the nano-grinding conditions are different: the solid-liquid mass volume ratio is 1g:10mL, ethanol is used as the medium, 0.3 and 0.5mm grinding beads are added to the original 0.05mm grinding beads to achieve a 3:4:3 ratio, and the grinding time is set to 4h. At this time, the grinding activation degree is higher than that of Example 1, and the critical temperature of the reduction conversion path can reach below 400°C, and pure phase α″-Fe 16 N2, but the particle size is only about 100nm, which makes it difficult to realize the subsequent magnetization and pressing process of magnetic powder.

Claims

1. A large-sized, high-purity α″-Fe 16 N 2 Method for preparing iron nitride magnetic powder, Features: The following steps are involved: 1) The iron ore concentrate is sequentially subjected to high-pressure roller milling, nano-sand milling and drying treatment to obtain micron-sized fine-particle iron oxide powder; the conditions of the high-pressure roller mill are: the feed particle size of the iron ore concentrate is: 40~100µm, the roller spacing is 100~150µm, the roller pressure is 10~20MPa, and the number of high-pressure roller cycles is 1~5 times; the conditions of the nano-sand mill are: the diameter of the grinding beads is 0.05mm~0.5mm, the grinding speed is not less than 2000r / min, the grinding time does not exceed 30min, the grinding medium is water, and the solid-liquid mass volume ratio is 1g:0.5~3mL. The conditions of the drying treatment are: vacuum drying method, air pressure of 90~100KPa, temperature of 60~100℃; 2) hydrogen reduction of micron-sized fine-particle iron oxide powder to obtain porous active reduced iron powder; the hydrogen reduction temperature is controlled to be within 50° C. below the critical temperature of the reduction conversion path, wherein the critical temperature of the reduction conversion path refers to the temperature at the intersection of the iron oxide hydrogen reduction fork curve; 3) The porous active reduced iron powder is nitrided in an ammonia atmosphere to obtain α″-Fe 16 N 2 Iron nitride.

2. A large-sized high-purity α″-Fe according to claim 1 16 N 2 Method for preparing iron nitride magnetic powder, Features: The total iron content of the iron concentrate is above 71.5%.

3. A large-sized high-purity α″-Fe according to claim 1 or 2 16 N 2 Method for preparing iron nitride magnetic powder, Features: The particle size of the micron-sized fine-particle iron oxide powder is 10-30 μm, and the activated lattice size is 150-800 Å.

4. A large-sized high-purity α″-Fe according to claim 1 or 2 16 N 2 Method for preparing iron nitride magnetic powder, Features: The conditions for hydrogen reduction are: the temperature is 20-50° C. lower than the critical temperature of the reduction conversion path, and the time is 2-5 hours.

5. A large-sized high-purity α″-Fe according to claim 1 or 2 16 N 2 Method for preparing iron nitride magnetic powder, Features: The critical temperature of the reduction path conversion of the micron-sized fine-particle iron oxide powder to iron concentrate is reduced to 350-520° C. based on the activation effect of the high-pressure roller mill and the nano-sand mill.

6. A large-sized high-purity α″-Fe according to claim 1 or 2 16 N 2 Method for preparing iron nitride magnetic powder, Features: The nitriding conditions are as follows: the ammonia pressure is not higher than 0.5 MPa, the nitriding temperature is 170-195° C., and the time is 8-15 hours.

Citation Information

Patent Citations

  • Magnetorheological materials utilizing surface-modified particles

    CA2186955A1

  • Method and device for preparing iron nitride material by double promotion of nanocrystallization and strong magnetic field

    CN101607701A

  • Method for preparing micro-nano iron powder through hydrogen reduction of ultra-pure iron ore concentrate

    CN114713835A

  • Core-Shell Structured Nanoparticle having Hard-soft Magnetic Heterostructure, Magnet Prepared with Said Nanoparticle, and Preparing Method thereof

    KR1020130090241A

Cited By

  • Method and device for preparing polycrystalline iron nitride in batches

    CN122543161A

  • Preparation method of submicron flaky Fe4N magnetic wave-absorbing material

    CN122585957A

  • A method for preparing submicron-scale sheet-like Fe4N magnetic microwave absorbing material

    CN122585957B