Nanometer lithium manganese iron phosphate, preparation method thereof, battery positive electrode and battery

The preparation of nitrogen-doped carbon-titanium composite materials and in-situ titanium-doped lithium manganese iron phosphate positive electrode materials was solved through the template method, which solved the low conductivity and manganese dissolution of lithium manganese iron phosphate positive electrode materials, significantly improving the cycle life and conductivity Rate.

CN118954462APending Publication Date: 2024-11-15JIANGSU TIANHE ENERGY STORAGE CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411020929.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing lithium manganese iron phosphate positive electrode materials have low conductivity and manganese dissolution problems, resulting in poor cycle life.

Method used

Nanotitanium dioxide with uniform pore size was prepared by the template method, and nitrogen doping and carbon coating were carried out on its surface to form a nitrogen-doped carbon-titanium composite material, and the stoichiometric ratio was mixed with iron, manganese, lithium and phosphorus sources. After sand milling, spray drying and sintering, lithium manganese iron phosphate material is prepared to achieve in-situ titanium doping and surface carbon coating, inhibit manganese dissolution and improve electrical conductivity.

Benefits of technology

The electronic and ionic conductivity of lithium manganese iron phosphate is significantly improved, the cycle life is extended, the manganese dissolution problem is avoided, and the particle size of the material is adjustable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954462A_ABST
    Figure CN118954462A_ABST
Patent Text Reader

Abstract

The invention discloses nano lithium manganese iron phosphate, a preparation method thereof, a battery positive electrode and a battery, porous nano titanium dioxide is prepared through a template method, and carbon coating is performed on the surface of titanium dioxide to form a carbon-titanium porous network structure; the lithium manganese iron phosphate precursor is further combined with the carbon-titanium porous network structure, surface carbon coating of the lithium manganese iron phosphate is achieved through porous carbon on the outer layer, bulk phase doping of the lithium manganese iron phosphate is achieved through titanium dioxide on the inner layer, and the lithium manganese iron phosphate grain growth process is limited in the porous carbon network structure; the problem that primary particles grow up in the sintering process is avoided, the size of the primary particles of the lithium manganese iron phosphate material is adjustable, the conductivity and rate capability of the lithium manganese iron phosphate are improved, the problem of manganese dissolution of the lithium manganese iron phosphate is inhibited, and the cycle life is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery positive electrode materials, and in particular to a nano-lithium manganese iron phosphate, a preparation method thereof, a battery positive electrode and a battery. Background Art

[0002] Lithium transition metal oxides are layered LiMO 2 (M=Co,Ni,Mn) and spinel LiMn 2 O 4 Olivine LiMPO is a representative material that has been used as the main cathode material for commercial lithium-ion batteries (LIBs). 4 (M=Fe, Mn, Co, etc.) has become a substitute for traditional oxide positive electrode materials.

[0003] Among them, LiFePO 4 (LFP) has attracted much attention due to its low cost, environmental friendliness, and thermal stability of strong PO bonds. The inherent low conductivity problem of LFP has been successfully solved by synthesizing nanoscale particles and coating them with carbon on the surface.

[0004] However, LFP has a lower working potential (3.4 V vs. Li / Li + ) and low energy density limit their application in electric vehicles such as hybrid electric vehicles (HEV) and plug-in HEV (PHEV). Lithium iron phosphate crystals are olivine-type, and the basic structural unit is LiO 6 Octahedron, LiO 6 Octahedron and PO 4 Tetrahedral composition, of which LiO 6 Octahedron and PO 6 Tetrahedral cross-linking forms a polyanion framework structure. + Transmission along a single b-axis. Lithium manganese iron phosphate adds Mn element to the structure of lithium iron phosphate, but it is not LiFePO 4 With LiMnPO 4 Simple physical mixing of Fe 2+ With Mn 2+ The ionic radius of LiFePO 4 With LiMnPO 4 The synergistic effect between them forms a stable and uniform solid solution, thereby converting LiFePO 4 Stable electrochemical performance and LiMnPO 4 combined with high potential.

[0005] The Mn element can increase the discharge voltage to 4.1V, greatly improving the energy density of the positive electrode material. Compared with lithium iron phosphate, lithium manganese iron phosphate has two main advantages-increased energy density and excellent low-temperature performance. Due to the higher voltage platform of Mn and the better conductivity of Fe, different manganese-iron ratios make the performance of lithium manganese iron phosphate different. When the manganese-iron ratio is high, Mn drives the battery voltage and energy density to increase significantly, but excessive manganese content will destroy the solid solution structure due to the Jahn-Teller effect, resulting in the dissolution of active materials and rapid decay of cycle performance. In order to give full play to the performance advantages of lithium manganese iron phosphate, the Mn content in the material is often not less than 50%, and the research on manganese-iron ratio is mainly concentrated in 5:5, 6:4, 7:3, 8:2 or 9:1. Most of the products currently under development are 64 or 73. The manganese content of Dangsheng Technology's lithium manganese iron phosphate product is 65%, and its patented manganese content covers a range of 40% to 90%; Rongke Technology has released a product with a phosphorus-manganese-iron ratio of 7:3, and has achieved stable mass production of 100 tons; the research range of Litai Lithium Energy's patented manganese content is 60% to 80%, which shows that high manganese-iron ratio is the direction of future efforts.

[0006] Lithium manganese iron phosphate and lithium iron phosphate have similar physical and chemical properties and problems such as low ionic and electronic conductivity. Therefore, the improvement methods used are similar. The main modification methods include nano-sizing, carbon coating and metal ion doping. Each technology can effectively improve the electrochemical properties of the material and meet the market commercialization needs.

[0007] However, the lithium manganese iron phosphate produced by the existing technical solutions still has many fatal defects, such as low electrical conductivity (insulator characteristics) and manganese dissolution (Jiang-Taylor effect, structural irreversibility, damage to the SEI film); therefore, how to inhibit the manganese dissolution of lithium manganese iron phosphate and improve the electronic / ionic conductivity of lithium manganese iron phosphate is still a technical problem currently faced by this field. Summary of the invention

[0008] The purpose of the present invention is to provide a nano-lithium manganese iron phosphate, a preparation method thereof, a battery positive electrode and a battery, so as to solve the manganese dissolution problem of lithium manganese iron phosphate and improve the cycle life.

[0009] In order to achieve the above-mentioned object of the invention, the present invention provides a method for preparing a nano-manganese iron phosphate lithium positive electrode material, comprising the following steps:

[0010] Adding the template to the first solvent, stirring evenly, and then adding to the first acid solution, adjusting the system solution to acidity, to obtain a first mixed solution;

[0011] Adding a titanium source to the first mixed solution, stirring uniformly at a first temperature to obtain a second mixed solution; inducing a gelation reaction of the second mixed solution at a second temperature, washing, drying at a third temperature to obtain a titanium dioxide xerogel, and calcining at a fourth temperature to obtain a titanium dioxide material with uniform pore size;

[0012] The titanium dioxide material, the first carbon source, the nitrogen source and the second acid solution obtained by calcination are stirred uniformly at a fifth temperature, and a three-stage high temperature treatment is performed to obtain a nitrogen-doped carbon-titanium composite material with uniform pore size;

[0013] Adding the prepared nitrogen-doped carbon-titanium composite material, an iron source, a manganese source, a lithium source, a phosphorus source and a second carbon source into a second solvent, and stirring evenly at room temperature to obtain a first slurry;

[0014] The first slurry is processed to obtain lithium manganese iron phosphate powder;

[0015] The lithium iron manganese phosphate powder is crushed to obtain a nano lithium iron manganese phosphate positive electrode material with a D50 of 20 to 100 nm.

[0016] Optionally, the template agent includes one of a polyethylene oxide-polypropylene oxide-polyethylene oxide PEO-PPO-PEO triblock copolymer, a polyethylene glycol-polypropylene oxide-polyethylene glycol PEG-PPO-PEG triblock copolymer, or a polyethylene glycol-polypropylene glycol-polyethylene glycol PEG-PPG-PEG triblock copolymer;

[0017] The titanium source includes: one of tetrabutyl titanate, tetraethyl titanate, tetrapropyl titanate, tetraisopropyl titanate or titanium tetrachloride;

[0018] The molar ratio of the template to the titanium source is (1.5-3):1.

[0019] Optionally, the concentration of the first acid solution is 0.2-3.0 mol / L; and the pH of the system solution is adjusted to 1-2.

[0020] Optionally, the first acid solution includes one or a combination of two of sulfuric acid, hydrochloric acid, nitric acid, phosphoric acid, acetic acid, citric acid, formic acid or oxalic acid.

[0021] Optionally, the first solvent includes: one of deionized water, ethanol, propanol, butanol or dichloromethane; the second solvent includes: one of deionized water, ethanol, and methanol.

[0022] Optionally, the concentration of the second acid solution is 0.5 to 2.5 mol / L;

[0023] The second acid solution includes one or a combination of sulfuric acid, hydrochloric acid, nitric acid or phosphoric acid.

[0024] Optionally, the first carbon source includes one or more combinations of sucrose, glucose or citric acid; the nitrogen source includes one or more combinations of ammonium phosphate, melamine, dopamine, urea or glycine.

[0025] Optionally, the particle size of the nitrogen-doped carbon-titanium composite material is 20-100 nm.

[0026] Optionally, the iron source includes one of ferric phosphate, ferrous oxalate or ferric nitrate; the manganese source includes one or more combinations of manganese phosphate, manganese nitrate, manganese sulfate or manganese acetate; the lithium source includes one or more combinations of lithium carbonate, lithium hydroxide, lithium nitrate or lithium dihydrogen phosphate; the phosphorus source includes one of phosphoric acid, lithium dihydrogen phosphate or ferric phosphate; the second carbon source includes one or more combinations of sucrose, glucose, polyethylene glycol 800, polyethylene glycol 2000, polyethylene glycol 4000, polyethylene glycol 6000 or citric acid.

[0027] Optionally, the molar ratio of lithium element to iron element is 1 to 1.2; the molar ratio of iron element to phosphorus element is 0.96 to 0.98; and the molar ratio of manganese element to iron element is 1.0 to 4.0.

[0028] Optionally, the first temperature is 35-50°C, and the stirring time is 0.5-2h; the second temperature is 100-130°C, and the mixture is allowed to stand in an oven at the second temperature for 24-48h; the third temperature is 80-100°C, and the mixture is dried in an oven at the third temperature for 24h; the fourth temperature is 500-650°C, and the mixture is calcined in an air environment for 4-8h.

[0029] Optionally, the fifth temperature is 35-50° C., and the stirring time is 2-6 hours.

[0030] Optionally, the three-stage high-temperature treatment includes: drying at a sixth temperature of 80 to 120°C for 16 to 24 hours; high-temperature pretreatment at a seventh temperature of 150 to 200°C; calcination at an eighth temperature of 600 to 900°C in an argon environment for 1 to 5 hours.

[0031] Optionally, the first slurry is transferred into a sand mill at a sand milling speed of 2000 to 5000 r / min for a sand milling time of 100 to 500 min until 20≤D50≤200 nm, to obtain the second slurry;

[0032] The second slurry is spray-dried by a centrifugal spray dryer, the inlet temperature is adjusted to 200-240° C., the outlet temperature is controlled to 80-90° C., and the feed rate is controlled to 5-10 mL / min to obtain spray-dried lithium iron manganese phosphate solid.

[0033] Optionally, the obtained lithium iron manganese phosphate solid is flattened and transferred to a box furnace, evacuated and introduced with high-purity nitrogen, and sintered to obtain lithium iron manganese phosphate powder;

[0034] The sintering process is provided with a low temperature heating section, a high temperature constant temperature section and a natural cooling section, wherein the low temperature heating section is heated from 80°C to the temperature set in the high temperature constant temperature section, and the heating rate is 1-10°C / min;

[0035] The high temperature constant temperature section is set at a temperature of 680-750° C., and the constant temperature time is 5-12 hours.

[0036] The present invention also provides a nano-lithium manganese iron phosphate material, comprising lithium manganese iron phosphate coated with porous carbon on the surface and in-situ titanium doped in the inner layer and dispersed in the porous carbon pore network structure.

[0037] The present invention also provides a battery positive electrode, which includes the nano-lithium manganese iron phosphate positive electrode material prepared by the above-mentioned method for preparing the nano-lithium manganese iron phosphate positive electrode material, or includes the above-mentioned nano-lithium manganese iron phosphate material.

[0038] The present invention also provides a battery, comprising the battery positive electrode as described above.

[0039] The invention prepares nano titanium dioxide with uniform pore size by a template method, and then forms a nitrogen-doped carbon-titanium composite material with uniform pore size, wherein the inner layer is titanium dioxide and the outer layer is a nitrogen-doped carbon layer, by in-situ coating of surface carbon and nitrogen doping, thereby significantly improving electronic conductivity and ionic conductivity; secondly, the prepared nitrogen-doped carbon-titanium composite material is mixed with an iron source, a manganese source, a lithium source and a second carbon source according to a stoichiometric ratio, and the lithium iron manganese phosphate material is obtained by sand milling, spray drying and sintering. In this process, the primary particles of the lithium iron manganese phosphate are restricted in the above network structure by means of the prepared nitrogen-doped carbon-titanium composite material with uniform pore size, the titanium dioxide in the inner layer is bulk-doped to ensure in-situ titanium doping of the lithium iron manganese phosphate, the outer layer is coated with surface carbon to avoid the problem of primary particle growth during sintering, so that the primary particle size of the lithium iron manganese phosphate material can be adjusted, and the manganese dissolution problem of the lithium iron manganese phosphate is suppressed, thereby improving the cycle life. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is a flow chart of the preparation method of nano-manganese iron phosphate lithium positive electrode material in an embodiment of the present invention;

[0041] Figure 2 This is an electron microscope photo of the nano-lithium manganese iron phosphate material prepared in Comparative Example 1 of the embodiment of the present invention;

[0042] Figure 3This is an electron microscope photograph of the nano-lithium manganese iron phosphate material prepared in Experimental Example 3 of the embodiment of the present invention. DETAILED DESCRIPTION

[0043] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] The serial numbers of the components herein, such as "first", "second", etc., are only used to distinguish the objects described and do not have any order or technical meaning. The "connection" and "coupling" mentioned in this application, unless otherwise specified, include direct and indirect connections (couplings). In the description of the present invention, it should be understood that the orientation or positional relationship indicated by the terms "upper", "lower", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", etc. are based on the orientation or positional relationship shown in the accompanying drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation to the present invention.

[0045] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0046] The present invention is described in more detail in the following paragraphs by way of example with reference to the accompanying drawings. The advantages and features of the present invention will become more apparent from the following description and claims. It should be noted that the drawings are in very simplified form and in non-precise proportions, and are only used to facilitate and clearly assist in illustrating the purpose of the embodiments of the present invention.

[0047] Please refer to Figure 1 This embodiment provides a method for preparing a nano-manganese iron phosphate lithium positive electrode material, comprising the following steps:

[0048] S1, adding the template to the first solvent, stirring evenly, and then adding to the first acid solution, adjusting the system solution to acidity, to obtain a first mixed solution;

[0049] S2, adding a titanium source to the first mixed solution, and stirring evenly at the first temperature to obtain a second mixed solution;

[0050] S3, inducing a gelation reaction of the second mixed solution at a second temperature, washing, drying at a third temperature to obtain a titanium dioxide xerogel, and calcining at a fourth temperature to obtain a titanium dioxide material with uniform pore size;

[0051] S4, stirring the calcined titanium dioxide material, the first carbon source, the nitrogen source and the second acid solution at a fifth temperature, and performing a three-stage high temperature treatment to obtain a nitrogen-doped carbon-titanium composite material with uniform pore size;

[0052] S5, adding the prepared nitrogen-doped carbon-titanium composite material, an iron source, a manganese source, a lithium source, a phosphorus source, and a second carbon source into a second solvent, and stirring evenly at room temperature to obtain a first slurry;

[0053] S6, treating the first slurry to obtain lithium manganese iron phosphate powder;

[0054] S7, crushing the lithium iron manganese phosphate powder to obtain a nano lithium iron manganese phosphate positive electrode material with a D50 of 20 to 100 nm.

[0055] In this embodiment, nano-titanium dioxide with uniform pore size is prepared by a template method, and then in-situ coating of surface carbon and nitrogen doping are performed to form a nitrogen-doped carbon-titanium composite material with uniform pore size, wherein the inner layer is titanium dioxide and the outer layer is a nitrogen-doped carbon layer, thereby significantly improving the electronic conductivity and ionic conductivity; secondly, the prepared nitrogen-doped carbon-titanium composite material is mixed with an iron source, a manganese source, a lithium source, and a second carbon source in a stoichiometric ratio, and the lithium iron manganese phosphate material is obtained after sand milling, spray drying, sintering, and the like. In this step, the primary particles of the lithium iron manganese phosphate are confined in a network structure with the help of the prepared nitrogen-doped carbon-titanium composite material with uniform pore size, the titanium dioxide in the inner layer is bulk-doped to ensure the in-situ titanium doping of the lithium iron manganese phosphate, and the outer layer is coated with surface carbon to avoid the problem of primary particle growth during the sintering process, so that the primary particle size of the lithium iron manganese phosphate material can be adjusted, and the manganese dissolution problem of the lithium iron manganese phosphate is suppressed, thereby improving the cycle life.

[0056] Specifically, the template agent includes one of P123 (polyethylene oxide-polypropylene oxide-polyethylene oxide PEO-PPO-PEO triblock copolymer), F127 (polyethylene glycol-polypropylene oxide-polyethylene glycol PEG-PPO-PEG triblock copolymer) or F108 (polyethylene glycol-polypropylene glycol-polyethylene glycol PEG-PPG-PEG triblock copolymer); preferably, the template agent is P123 (polyethylene oxide-polypropylene oxide-polyethylene oxide PEO-PPO-PEO triblock copolymer).

[0057] The titanium source includes: one of tetrabutyl titanate, tetraethyl titanate, tetrapropyl titanate, tetraisopropyl titanate or titanium tetrachloride; preferably, the titanium source is tetrabutyl orthotitanate.

[0058] Furthermore, the molar ratio of the template to the titanium source is (1.5-3):1.

[0059] Further, in step S1, the concentration of the first acid solution is 0.2-3.0 mol / L; preferably, the concentration of the first acid solution is 2.0-2.5 mol / L.

[0060] Furthermore, the pH of the system solution is adjusted to 1-2.

[0061] The first acid solution includes one or a combination of two of sulfuric acid, hydrochloric acid, nitric acid, phosphoric acid, acetic acid, citric acid, formic acid or oxalic acid.

[0062] Furthermore, the first solvent includes: one of deionized water, ethanol, propanol, butanol or dichloromethane.

[0063] The second solvent includes: one of deionized water, ethanol and methanol.

[0064] Furthermore, in step S4, the concentration of the second acid solution is 0.5-2.5 mol / L.

[0065] The second acid solution includes one or a combination of two of sulfuric acid, hydrochloric acid, nitric acid or phosphoric acid.

[0066] Furthermore, the first carbon source includes one or more combinations of sucrose, glucose or citric acid; the nitrogen source includes one or more combinations of ammonium phosphate, melamine, dopamine, urea or glycine.

[0067] The particle size of the nitrogen-doped carbon-titanium composite material obtained in step S4 is 20-100 nm.

[0068] In step S5, the iron source includes one of ferric phosphate, ferrous oxalate or ferric nitrate; the manganese source includes one or more combinations of manganese phosphate, manganese nitrate, manganese sulfate or manganese acetate; the lithium source includes one or more combinations of lithium carbonate, lithium hydroxide, lithium nitrate or lithium dihydrogen phosphate; the phosphorus source includes one of phosphoric acid, lithium dihydrogen phosphate or ferric phosphate; the second carbon source includes one or more combinations of sucrose, glucose, polyethylene glycol 800, polyethylene glycol 2000, polyethylene glycol 4000, polyethylene glycol 6000 or citric acid.

[0069] Furthermore, the molar ratio of lithium element to iron element is 1 to 1.2; the molar ratio of iron element to phosphorus element is 0.96 to 0.98; and the molar ratio of manganese element to iron element is 1.0 to 4.0.

[0070] Furthermore, in the steps of the above preparation method, the first temperature is 35-50°C, and the stirring time is 0.5-2h; the second temperature is 100-130°C, and the mixture is allowed to stand in an oven at the second temperature for 24-48h; the third temperature is 80-100°C, and the mixture is dried in an oven at the third temperature for 24h; the fourth temperature is 500-650°C, and the mixture is calcined in an air environment for 4-8h.

[0071] Furthermore, the fifth temperature is 35-50°C, and the stirring time is 2-6h; the three-stage high-temperature treatment includes: drying at a sixth temperature of 80-120°C for 16-24h; high-temperature pretreatment at a seventh temperature of 8-16h; the seventh temperature is 150-200°C; calcination at an eighth temperature in an argon environment for 1-5h, and the eighth temperature is 600-900°C.

[0072] In step S6, the following steps are specifically included:

[0073] S61, transferring the first slurry into a sand mill at a sand milling speed of 2000-5000 r / min for a sand milling time of 100-500 min until 20≤D50≤200 nm, to obtain a second slurry;

[0074] S62, spray drying the second slurry using a centrifugal spray dryer, adjusting the inlet temperature to 200-240° C., controlling the outlet temperature to 80-90° C., and controlling the feed rate to 5-10 mL / min, to obtain a spray-dried lithium iron manganese phosphate solid;

[0075] S63, flattening the obtained lithium iron manganese phosphate solid and transferring it to a box-type furnace, evacuating the furnace and introducing high-purity nitrogen to sinter the furnace to obtain lithium iron manganese phosphate powder.

[0076] The sintering process is provided with a low-temperature heating section, a high-temperature constant temperature section and a natural cooling section. The low-temperature heating section is heated from 80°C to the temperature set in the high-temperature constant temperature section, and the heating rate is 1-10°C / min; the high-temperature constant temperature section is set at a temperature of 680-750°C, and the constant temperature time is 5-12h.

[0077] The present invention also provides a nano-lithium manganese iron phosphate material, which includes lithium manganese iron phosphate coated with porous carbon on the surface and in-situ titanium doped in the inner layer and dispersed in the porous carbon pore network structure.

[0078] The present invention also provides a battery positive electrode, which includes the nano-lithium manganese iron phosphate positive electrode material prepared by the above-mentioned method for preparing the nano-lithium manganese iron phosphate positive electrode material, or includes the above-mentioned nano-lithium manganese iron phosphate material.

[0079] The present invention also provides a battery, comprising the battery positive electrode as described above.

[0080] This embodiment also provides three groups of experimental examples and one group of comparative examples.

[0081] Experimental Example 1

[0082] (1) 16.6 g of template P123 was added to 100 g of deionized water, and then added to 400.0 g of 2.0 mol / L hydrochloric acid solution, stirred at 35°C for 1 hour, and the pH was adjusted to 1-2; 17.02 g of tetrabutyl titanate was added, and stirred at 35°C for 12 hours to obtain a uniform first mixed solution; then the mixture was transferred to an oven and kept at 110°C for 24 hours to obtain a gel; the gel was washed with deionized water and then dried at 100°C for 24 hours. In an air environment, the sample was calcined at 450°C for 6 hours to obtain a titanium dioxide material with a pore size of 50 nm.

[0083] (2) 8.0 g of the titanium dioxide material prepared above, 10.0 g of sucrose, and 4.0 g of ammonium phosphate were dissolved in deionized water, and then 4.00 g of a 2.0 mol / L hydrochloric acid solution was dripped into the solution to adjust the pH to 1-2; the mixture was stirred at room temperature for 2 h, and then dried at 100°C for 24 h, and pretreated at 160°C for 24 h. After drying, a 50 nm nitrogen-doped carbon-titanium composite material was obtained by high-temperature treatment (600°C / Ar atmosphere) for 2 h.

[0084] (3) 10.0 g of the 50 nm nitrogen-doped carbon-titanium composite material prepared above, 12.0 g of ferrous oxalate, 3.0 g of manganese oxalate, and 8.66 g of lithium dihydrogen phosphate were added to 100 g of deionized water in sequence, and stirred at room temperature for 1 hour to obtain a first slurry.

[0085] (4) The first slurry was transferred into a sand mill at a speed of 2000 r / min for 500 min. After the sand milling was completed, the particle size was measured using a Malvern 3000 particle size analyzer until D50 was 50 nm, thereby obtaining a second slurry.

[0086] (5) After sand milling, the second slurry was transferred to a beaker and spray dried using a centrifugal spray dryer. The inlet temperature was adjusted to 220°C, the outlet temperature was controlled to 80°C, and the feed rate was controlled to 8 mL / min. The outlet temperature was controlled to be stable according to the viscosity of the slurry and the feed rate. Finally, the spray-dried sample was collected in a sample collection bottle to obtain solid A.

[0087] (6) Transfer solid A to a graphite crucible, flatten the powder, and further transfer it to a box furnace. Before heating, evacuate the furnace, introduce high-purity nitrogen, and heat the furnace to 700°C at a heating rate of 10°C / min and sinter for 10 hours to obtain lithium manganese iron phosphate material.

[0088] (7) The powder obtained above is crushed by a jet mill to obtain the final product - a nano-manganese iron phosphate lithium positive electrode material with a primary particle size of 50 nm.

[0089] Experimental Example 2

[0090] (1) 30 g of template F127 was added to 100 g of deionized water and 14.49 g of acetic acid, stirred at 35 ° C for 1 hour, and the pH was adjusted to 2-3; 17.87 g of tetrabutyl titanate was added, and stirred at 35 ° C for 12 hours to obtain a uniform first mixed solution; the mixture was then transferred to an oven and kept at 120 ° C for 36 hours to obtain a gel; the gel was washed with deionized water and then dried at 100 ° C for 24 hours. The sample was calcined at 600 ° C for 6 hours in an air environment to obtain a titanium dioxide material with a pore size of 60 nm.

[0091] (2) 6.0 g of the titanium dioxide material prepared above, 5.0 g of glucose, and 2.0 g of ammonium phosphate were dissolved in deionized water, and then 2 g of sulfuric acid was dropped into the solution to adjust the pH to acidic. Stir at 35°C for 1 h, then dry at 80°C for 24 h, and pre-treat at 180°C for 24 h. After drying, high-temperature treatment (600°C / Ar atmosphere) for 2 h was performed to obtain a 60 nm nitrogen-doped carbon-titanium composite material.

[0092] (3) 5.0 g of the 60 nm nitrogen-doped carbon-titanium composite material prepared above, 2.0 g of PEG6000, 6.0 g of ferrous oxalate, 1.49 g of manganese oxalate, 0.078 g of lithium carbonate, and 4.20 g of lithium phosphate were added to 80 g of methanol in sequence, and stirred at room temperature for 1 hour to obtain a first slurry.

[0093] (4) The first slurry was transferred into a sand mill at a speed of 2000 r / min for 400 min. After the sand milling was completed, the particle size was measured using a Malvern 3000 particle size analyzer until D50 was 100 nm, thereby obtaining a second slurry.

[0094] (5) After sand milling, the second slurry was transferred to a beaker and spray dried using a centrifugal spray dryer. The inlet temperature was adjusted to 220°C, the outlet temperature was controlled to 80°C, and the feed rate was controlled to 8 mL / min. The outlet temperature was controlled to be stable according to the viscosity of the slurry and the feed rate. Finally, the spray-dried sample was collected in a sample collection bottle to obtain solid A.

[0095] (6) Transfer solid A to a graphite crucible, flatten the powder, and further transfer it to a box furnace. Before heating, evacuate the furnace, introduce high-purity nitrogen, and heat the furnace to 680°C at a heating rate of 10°C / min and sinter for 10 hours to obtain lithium manganese iron phosphate material.

[0096] (7) The powder obtained above is crushed by a jet mill to obtain the final product - a nano-manganese iron phosphate lithium positive electrode material with a primary particle size of 60 nm.

[0097] Experimental Example 3

[0098] (1) 15g of template F127 was added to 80g of deionized water and then to 8g of sulfuric acid, stirred at 35°C for 2h, and the pH was adjusted to 3-4; 8.92g of tetraethyl titanate was added, and stirred at 35°C for 12h to obtain a uniform first mixed solution; the mixture was then transferred to an oven and kept at 130°C for 24h to obtain a gel; the gel was washed with deionized water and then dried at 90°C for 24h. The sample was calcined at 580°C for 5h in an air environment to obtain a titanium dioxide material with a pore size of 75nm.

[0099] (2) Dissolve 5.0 g of the titanium dioxide material prepared above, 5.0 g of glucose, and 2.0 g of melamine in deionized water, then drop 2 g of sulfuric acid into the solution to adjust the pH to acidic. Stir at 35°C for 1 h, then dry at 80°C for 24 h, and pre-treat at 180°C for 24 h. After drying, high-temperature treatment (600°C / Ar atmosphere) for 2 h was performed to obtain a 75 nm nitrogen-doped carbon-titanium composite material.

[0100] (3) 12.0 g of the 60 nm nitrogen-doped carbon-titanium composite material prepared above, 2.0 g of PEG6000, 15.0 g of ferrous nitrate, 6.39 g of manganese nitrate, and 8.41 g of lithium phosphate were added to 100 g of deionized water in sequence, and stirred at room temperature for 1 hour to obtain a first slurry.

[0101] (4) The first slurry was transferred into a sand mill at a speed of 1800 r / min for 600 min. After the sand milling was completed, the particle size was measured using a Malvern 3000 particle size analyzer until D50 was 100 nm, thereby obtaining a second slurry.

[0102] (5) After sand milling, the second slurry was transferred to a beaker and spray dried using a centrifugal spray dryer. The inlet temperature was adjusted to 220°C, the outlet temperature was controlled to 80°C, and the feed rate was controlled to 8 mL / min. The outlet temperature was controlled to be stable according to the viscosity of the slurry and the feed rate. Finally, the spray-dried sample was collected in a sample collection bottle to obtain solid A.

[0103] (6) Transfer solid A to a graphite crucible, flatten the powder, and further transfer it to a box furnace. Before heating, evacuate the furnace and introduce high-purity nitrogen. Heat the temperature to 710°C at a heating rate of 10°C / min and sinter for 9.5h to obtain lithium manganese iron phosphate material.

[0104] (7) The powder obtained above is crushed by a jet mill to obtain the final product - a nano-manganese iron phosphate lithium positive electrode material with a primary particle size of 75 nm.

[0105] Comparative Experiment 1

[0106] Experimental Example 3 was selected as a comparative experiment, in which the nitrogen-doped carbon-titanium composite material was not prepared, and other experimental conditions were the same as those described in Experimental Example 3.

[0107] (1) 2.0 g of PEG6000, 15.0 g of ferrous nitrate, 6.39 g of manganese nitrate, and 8.41 g of lithium phosphate were added to 100 g of deionized water in sequence, and stirred at room temperature for 1 hour to obtain a first slurry.

[0108] (2) The first slurry was transferred into a sand mill at a speed of 1800 r / min for 600 min. After the sand milling was completed, the particle size was measured using a Malvern 3000 particle size analyzer until D50 was 100 nm, thereby obtaining a second slurry.

[0109] (3) After sand milling, the second slurry was transferred to a beaker and spray dried using a centrifugal spray dryer. The inlet temperature was adjusted to 220°C, the outlet temperature was controlled to 80°C, and the feed rate was controlled to 8 mL / min. The outlet temperature was controlled to be stable according to the viscosity of the slurry and the feed rate. Finally, the spray-dried sample was collected in a sample collection bottle to obtain solid A.

[0110] (4) Transfer solid A to a graphite crucible, flatten the powder, and further transfer it to a box furnace. Before heating, evacuate the furnace and introduce high-purity nitrogen. Heat the temperature to 710°C at a heating rate of 10°C / min and sinter for 9.5h to obtain lithium manganese iron phosphate material.

[0111] (5) The powder obtained above is crushed by a jet mill to obtain the final product. The particle size of the lithium manganese iron phosphate material is: D50 is 0.9 μm, and 60% of the primary particles are mostly concentrated between 100 and 200 nm, and the size of some primary particles exceeds 200 nm. Please refer to Figure 2 , obvious agglomeration occurred.

[0112] Please refer to Figure 3 In Experimental Example 3, the prepared carbon-titanium composite material is a porous material with a pore size between 20 and 100 nm. Due to its high specific surface area, it exhibits uniform pore size and developed pore channels.

[0113] In this comparative example 1, due to the lack of preparation of carbon-titanium composite materials, the size control effect of the primary particles of the prepared lithium manganese iron phosphate is not as good as that of experimental example 3, and the requirement of improving the material rate performance cannot be met.

[0114] In summary, the present invention proposes a method for preparing a nano-lithium iron manganese phosphate positive electrode material. The present invention discloses a method for preparing a nano-lithium iron manganese phosphate positive electrode material, which prepares the surface coating of nitrogen-doped porous carbon and in-situ titanium doping of lithium iron manganese phosphate by a template method, so that the primary particle size of the lithium iron manganese phosphate material can be adjusted, the conductivity is improved, and the manganese dissolution problem of lithium iron manganese phosphate can be suppressed, thereby improving the cycle life.

[0115] Obviously, the above embodiments are only illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by those with ordinary knowledge in the relevant technical field without departing from the spirit and technical ideas disclosed by the present invention should still be covered by the claims of the present invention.

Claims

1. A method for preparing nano-manganese iron phosphate lithium positive electrode material, characterized in that: The following steps are involved: Adding the template to the first solvent, stirring evenly, and then adding to the first acid solution, adjusting the system solution to acidity, to obtain a first mixed solution; Adding a titanium source to the first mixed solution, and stirring uniformly at a first temperature to obtain a second mixed solution; Inducing a gelation reaction of the second mixed solution at a second temperature, washing and drying at a third temperature to obtain a titanium dioxide xerogel, and calcining at a fourth temperature to obtain a titanium dioxide material with uniform pore size; The titanium dioxide material, the first carbon source, the nitrogen source and the second acid solution obtained by calcination are stirred uniformly at a fifth temperature, and a three-stage high temperature treatment is performed to obtain a nitrogen-doped carbon-titanium composite material with uniform pore size; Adding the prepared nitrogen-doped carbon-titanium composite material, an iron source, a manganese source, a lithium source, a phosphorus source and a second carbon source into a second solvent, and stirring evenly at room temperature to obtain a first slurry; The first slurry is processed to obtain lithium manganese iron phosphate powder; The lithium iron manganese phosphate powder is crushed to obtain a nano lithium iron manganese phosphate positive electrode material with a D50 of 20 to 100 nm.

2. The method for preparing the nano-manganese iron lithium phosphate positive electrode material according to claim 1, characterized in that: The template agent includes one of a polyethylene oxide-polypropylene oxide-polyethylene oxide PEO-PPO-PEO triblock copolymer, a polyethylene glycol-polypropylene oxide-polyethylene glycol PEG-PPO-PEG triblock copolymer or a polyethylene glycol-polypropylene glycol-polyethylene glycol PEG-PPG-PEG triblock copolymer; The titanium source includes: one of tetrabutyl titanate, tetraethyl titanate, tetrapropyl titanate, tetraisopropyl titanate or titanium tetrachloride; The molar ratio of the template to the titanium source is (1.5-3):

1.

3. The method for preparing the nano-manganese iron lithium phosphate positive electrode material according to claim 1, characterized in that: The concentration of the first acid solution is 0.2-3.0 mol / L; and the pH of the system solution is adjusted to 1-2.

4. The method for preparing the nano-manganese iron lithium phosphate positive electrode material according to claim 1, characterized in that: The first acid solution includes one or a combination of two of sulfuric acid, hydrochloric acid, nitric acid, phosphoric acid, acetic acid, citric acid, formic acid or oxalic acid.

5. The method for preparing the nano-manganese iron lithium phosphate positive electrode material according to claim 1, characterized in that: The first solvent includes: one of deionized water, ethanol, propanol, butanol or dichloromethane; the second solvent includes: one of deionized water, ethanol, methanol.

6. The method for preparing the nano-manganese iron lithium phosphate positive electrode material according to claim 1, characterized in that: The concentration of the second acid solution is 0.5 to 2.5 mol / L; The second acid solution includes one or a combination of two of sulfuric acid, hydrochloric acid, nitric acid or phosphoric acid.

7. The method for preparing the nano-manganese iron lithium phosphate positive electrode material according to claim 1, characterized in that: The first carbon source includes one or more combinations of sucrose, glucose or citric acid; the nitrogen source includes one or more combinations of ammonium phosphate, melamine, dopamine, urea or glycine.

8. The method for preparing the nano-manganese iron lithium phosphate positive electrode material according to claim 1, characterized in that: The particle size of the nitrogen-doped carbon-titanium composite material is 20-100 nm.

9. The method for preparing the nano-manganese iron lithium phosphate positive electrode material according to claim 1, characterized in that: The iron source includes one of ferric phosphate, ferrous oxalate or ferric nitrate; the manganese source includes one or more combinations of manganese phosphate, manganese nitrate, manganese sulfate or manganese acetate; the lithium source includes one or more combinations of lithium carbonate, lithium hydroxide, lithium nitrate or lithium dihydrogen phosphate; the phosphorus source includes one of phosphoric acid, lithium dihydrogen phosphate or ferric phosphate; the second carbon source includes one or more combinations of sucrose, glucose, polyethylene glycol 800, polyethylene glycol 2000, polyethylene glycol 4000, polyethylene glycol 6000 or citric acid.

10. The method for preparing the nano-manganese iron lithium phosphate positive electrode material according to claim 1, characterized in that: The molar ratio of lithium element to iron element is 1-1.2; the molar ratio of iron element to phosphorus element is 0.96-0.98; and the molar ratio of manganese element to iron element is 1.0-4.

0.

11. The method for preparing the nano-manganese iron lithium phosphate positive electrode material according to claim 1, characterized in that: The first temperature is 35-50°C, and the stirring time is 0.5-2h; the second temperature is 100-130°C, and the mixture is allowed to stand in an oven at the second temperature for 24-48h; the third temperature is 80-100°C, and the mixture is dried in an oven at the third temperature for 24h; the fourth temperature is 500-650°C, and the mixture is calcined in an air environment for 4-8h.

12. The method for preparing the nano-manganese iron lithium phosphate positive electrode material according to claim 1, characterized in that: The fifth temperature is 35-50° C., and the stirring time is 2-6 hours.

13. The method for preparing nano-manganese iron lithium phosphate positive electrode material according to claim 1, characterized in that: The three-stage high-temperature treatment includes: drying at a sixth temperature of 80 to 120°C for 16 to 24 hours; high-temperature pretreatment at a seventh temperature of 150 to 200°C; calcination at an eighth temperature of 600 to 900°C in an argon environment for 1 to 5 hours.

14. The method for preparing nano-manganese iron phosphate lithium positive electrode material according to claim 1, characterized in that: The first slurry is transferred into a sand mill at a sand milling speed of 2000 to 5000 r / min for a sand milling time of 100 to 500 min until 20 ≤ D50 ≤ 200 nm, to obtain the second slurry; The second slurry is spray-dried by a centrifugal spray dryer, the inlet temperature is adjusted to 200-240° C., the outlet temperature is controlled to 80-90° C., and the feed rate is controlled to 5-10 mL / min to obtain spray-dried lithium iron manganese phosphate solid.

15. The method for preparing nano-manganese iron lithium phosphate positive electrode material according to claim 14, characterized in that: The obtained lithium iron manganese phosphate solid is flattened and transferred to a box furnace, evacuated and introduced with high-purity nitrogen to sinter to obtain lithium iron manganese phosphate powder; The sintering process is provided with a low temperature heating section, a high temperature constant temperature section and a natural cooling section, wherein the low temperature heating section is heated from 80°C to the temperature set in the high temperature constant temperature section, and the heating rate is 1-10°C / min; The high temperature constant temperature section is set at a temperature of 680-750° C., and the constant temperature time is 5-12 hours.

16. A nano-manganese iron lithium phosphate material, characterized in that: It includes lithium manganese iron phosphate with a porous carbon coating on the surface and in-situ titanium doping in the inner layer and dispersed in the porous carbon pore network structure.

17. A positive electrode of a battery, characterized in that: The positive electrode comprises the nano-lithium manganese iron phosphate positive electrode material prepared by the method for preparing the nano-lithium manganese iron phosphate positive electrode material according to any one of claims 1 to 15, or comprises the nano-lithium manganese iron phosphate material according to claim 16.

18. A battery, characterized in that: The battery comprises the battery positive electrode according to claim 17.

Citation Information

Patent Citations

  • Lithium manganese iron phosphate positive electrode material, positive electrode, lithium ion battery and preparation method

    CN114975990A

  • Nanometer titanium dioxide network composite mesoporous carbon coated lithium manganese iron phosphate and preparation method thereof

    CN116706003A

  • Preparation method of doped lithium iron manganese phosphate positive electrode material

    CN117886289A

  • Composite positive electrode material and preparation method and application thereof

    CN118239459A