Graphite composite material and preparation method and application thereof

By doping graphene and catalyst in the graphite anode material of lithium-ion batteries and deposition of amorphous carbon by vapor deposition, the problem of taking into account the energy density and fast charging performance of the material is solved, and the conductivity of the material is significantly improved. Cycling performance improves battery charge and discharge efficiency and safety.

CN118954498AActive Publication Date: 2024-11-15SHENZHEN GOLD MEDAL NEW ENERGY TECH CO LTD +1

Patent Information

Application Number
CN202411232447.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-15
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

The graphite anode materials of existing lithium-ion batteries are difficult to balance between energy density and fast charging performance, which leads to an increase in the energy density of the material to reduce the fast charging performance, and vice versa, and there are challenges in the circulation and safety of the material.

Method used

By doping graphene and catalyst in raw material coke and graphitizing at high temperature, combined with vapor deposition method to deposit heteroatom amorphous carbon, the compaction density, specific surface area and electron conductivity of the material are improved, and the lithium ions are shortened. Embed the path and improve fast charging performance.

Benefits of technology

It significantly improves the powder conductivity, discharge specific capacity, magnification and cycling performance of graphite composite materials, improves fast charging performance and first-time efficiency, reduces material expansion, enhances the transmission path of lithium ions, and optimizes the charging and discharge of batteries. process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954498A_ABST
    Figure CN118954498A_ABST
Patent Text Reader

Abstract

The invention discloses a graphite composite material and a preparation method and application thereof, and the preparation method of the graphite composite material comprises the following steps: carrying out melting treatment on crushed raw material coke, a catalyst, graphene and a binder to obtain a mixture, and then carrying out hot pressing on the mixture to obtain briquetting graphite; sequentially carrying out pre-carbonization, low-temperature graphitization treatment and high-temperature graphitization treatment on the briquetting graphite to obtain a graphite material; and carrying out heat treatment on the graphite material under the condition of introducing a heteroatom-containing carbon source gas to obtain the graphite composite material. According to the preparation method of the graphite composite material, the raw material coke is doped with the graphene and the catalyst, and the compaction density of the material is improved by means of high electronic conductivity and high ductility of the graphene; the nano-pores left by high-temperature volatilization of the catalyst can also increase the specific surface area of the material, shorten the transmission path of lithium ions in the charge-discharge process and improve the fast charge performance of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of secondary batteries, and in particular to a method for preparing a graphite composite material, the graphite composite material and applications thereof. Background Art

[0002] As a green and environmentally friendly new energy, lithium-ion batteries have the advantages of good reliability, high safety, small size and light weight. They have been widely used in digital products, electric vehicles, military products and other fields. With the vigorous development of the new energy industry, the development of lithium-ion batteries is in full swing, but the requirements for the service life, safety and low cost of lithium-ion batteries are also getting higher and higher. At present, lithium-ion batteries are also developing in the direction of long life, high safety, high rate and low cost.

[0003] The negative electrode material is one of the key factors that restrict the energy density and rate charge and discharge performance of lithium-ion batteries. The negative electrode materials used in energy storage batteries are mainly selected from raw materials with high isotropy, artificial graphite materials with low specific surface area and low expansion. However, as the new SEI film expands during the cycle, it consumes lithium ions, causing the cycle performance to decrease during the charge and discharge process.

[0004] Compared with natural graphite negative electrode materials, artificial graphite negative electrode materials have better performance, and artificial graphite negative electrode materials have become the mainstream of power battery negative electrode materials. At present, the raw materials used to prepare artificial graphite lithium-ion battery negative electrode materials are mainly raw coke, including: needle coke, petroleum coke, and asphalt coke.

[0005] As the market's requirements for lithium-ion battery energy density and fast-charging performance increase, the graphite negative electrode materials used in lithium-ion batteries are required to have high specific capacity, compaction density and excellent fast-charging performance. However, it is difficult for the currently commercialized graphite negative electrode materials to simultaneously improve both energy density and fast-charging performance. The reason is that the energy density of graphite is improved mainly by increasing the degree of graphitization and increasing the particle size, but this will reduce the fast-charging performance of the material. The fast-charging performance is improved mainly by reducing the particle size, amorphous carbon coating and secondary granulation, which will also reduce the specific capacity, compaction density and initial efficiency of the material. Although researchers have improved the energy density of materials by doping silicon-based materials, this results in large expansion at full charge, reduced cycle performance and reduced electronic conductivity. Patent application No. CN202210609143.7 discloses a method for preparing a graphite negative electrode material with high energy density and fast charging for lithium batteries. The modified graphene is evenly distributed in the graphite phase through mixing, pressing and graphitization. The two have good contact performance, which greatly enhances the conductivity of the graphite material and its coating layer; secondly, catalytic graphitization can increase the capacity of graphite to more than 360mAh / g, further improving the energy density of the battery; the synergistic effect brought about by graphene modification and catalyst pore creation improves the fast charging performance, but catalytic graphitization brings about an increase in the specific surface area of ​​the material and an increase in the first efficiency, resulting in its low first efficiency. Although the number of internal pores in the material has increased, the isotropy of the material is poor, and the fast charging performance of the material is deviated. Summary of the invention

[0006] Based on this, it is necessary to provide a method for preparing a graphite composite material that can solve the above problems.

[0007] In addition, it is also necessary to provide a graphite composite material prepared by the preparation method of the graphite composite material and the application of the graphite composite material.

[0008] A method for preparing a graphite composite material comprises the following steps:

[0009] The crushed raw coke, catalyst, graphene and binder are melt-treated to obtain a mixture, and then the mixture is hot-pressed to obtain a briquetted graphite;

[0010] The compressed graphite is heated to 500-800°C for pre-carbonization for 1-6 hours, then heated to 2000-2500°C for low-temperature graphitization for 6 hours to 18 hours, and then heated to 3000-3200°C for high-temperature graphitization for 12 hours to 48 hours to obtain a graphite material;

[0011] The graphite material is heat treated under the condition of introducing carbon source gas containing heteroatoms to obtain a graphite composite material.

[0012] In one embodiment, in the operation of melting the crushed raw coke, catalyst, graphene and binder, the mass ratio of the raw coke, the catalyst, the graphene and the binder is 100:1-5:1-5:5-15.

[0013] In one embodiment, the binder is polyamide asphalt;

[0014] The polyamide asphalt is prepared by the following method: asphalt, amino acid anhydride and initiator are mixed evenly according to a mass ratio of 100:1-5:0.5-2, stirred at a temperature of 100°C-200°C and a speed of 500rpm-100rpm for 1h-4h, filtered and dried to obtain the polyamide asphalt.

[0015] In one embodiment, the amino acid anhydride is selected from at least one of 4-dimethylaminobenzoic anhydride, 3-dimethylaminobenzoic anhydride and 3-acetamidophthalic anhydride;

[0016] The initiator is selected from at least one of peracetic acid, peroxyacetic acid and perbenzoic acid.

[0017] In one embodiment, in the operation of melting the crushed raw coke, catalyst, graphene and binder, the temperature of the melting treatment is 300° C.-500° C., and the time of the melting treatment is 1 h-6 h;

[0018] In the operation of hot pressing the mixture, the pressure of the hot pressing is 20Mpa-50Mpa, the time of the hot pressing is 2h-4h, and the temperature of the hot pressing is 100°C-200°C.

[0019] In one embodiment, the raw coke is selected from at least one of petroleum coke, oil-based needle coke, coal-based needle coke and asphalt coke;

[0020] The catalyst is selected from at least one of nickel chloride, cupric chloride, ferric chloride, nickel powder, cobalt powder and iron powder.

[0021] In one embodiment, the graphite material is heat treated under the condition of passing a carbon source gas containing heteroatoms, the heat treatment temperature is 700°C-1000°C, the heat treatment time is 30min-300min, and the flow rate of the carbon source gas containing heteroatoms is 100ml / min-500ml / min.

[0022] In one embodiment, the carbon source gas containing heteroatoms is at least one of CF4, COF2, CH2O, C2F4H2 and CCl3F.

[0023] A graphite composite material is prepared by the above-mentioned graphite composite material preparation method.

[0024] Application of the above graphite composite materials in the field of energy storage devices.

[0025] The preparation method of the graphite composite material of the present invention increases the compaction density of the material by doping graphene into the raw coke, relying on the high electronic conductivity and high ductility of the graphene; at the same time, a catalyst is added to promote the graphitization reaction process. In addition, the nanopores left by the high-temperature volatilization of the catalyst can also increase the specific surface area of ​​the material and shorten the transmission path of lithium ions during the charging and discharging process and improve the fast charging performance of the material; at the same time, a binder is doped into the material, and after the binder is carbonized, the isotropy of the material is improved, the expansion is reduced, the insertion and extraction path of lithium ions during the charging and discharging process is shortened, and the fast charging performance of the material is improved.

[0026] In addition, the preparation method of the graphite composite material of the present invention deposits heteroatom-doped amorphous carbon on the surface of the graphite material by vapor deposition. Compared with traditional liquid phase and solid phase coating methods, it has the advantages of good coating uniformity, high electronic conductivity, and reduction of the specific surface area of ​​the inner core of the prepared graphite composite material, thereby improving the fast charging performance and initial efficiency of the prepared graphite composite material.

[0027] In combination with specific embodiments, the powder conductivity and OI value of the graphite composite material prepared by the preparation method of the graphite composite material of the present invention are significantly better than those of the comparative example. The discharge specific capacity, rate and cycle performance of the negative electrode sheet prepared using this graphite composite material are significantly higher than those of the comparative example. The rate charging performance of the soft-pack battery prepared using this graphite composite material is significantly better than that of the comparative example, and the charging time is shorter, indicating that the composite negative electrode material of the present invention has good fast charging performance.

[0028] Preferably, in this embodiment, the binder is polyamide pitch. Polyamide pitch is mixed into the raw coke to improve the material's liquid retention performance and ion transmission path by virtue of the good isotropy, high electronic conductivity and micron-nano pores generated after carbonization of polyamide pitch.

[0029] In addition, polyamide asphalt can form an -OCO- structure and pores between graphite by relying on its own oxygen free radicals. The isotropy of polyamide asphalt formed after carbonization is high, which reduces expansion, shortens the insertion and extraction path of lithium ions during charging and discharging, and improves fast charging performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0031] in:

[0032] Figure 1 The present invention is a flow chart of a method for preparing a graphite composite material according to one embodiment.

[0033] Figure 2 This is the SEM image of the graphite composite material prepared in Example 1. DETAILED DESCRIPTION

[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] In the present invention, the descriptions involving "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0036] Combination Figure 1 The present invention discloses a method for preparing a graphite composite material according to an embodiment of the present invention, comprising the following steps:

[0037] S10, melting the crushed raw coke, catalyst, graphene and binder to obtain a mixture, and then hot pressing the mixture to obtain briquetted graphite.

[0038] Graphene, as a new type of two-dimensional layered carbon material, has a high aspect ratio and excellent hydrophobicity, thermal conductivity and chemical stability. The conjugated system makes its electronic conduction ability very strong and has excellent electrical conductivity.

[0039] By doping graphene into the raw coke, the compaction density of the material can be improved by relying on the high electronic conductivity and high ductility of graphene.

[0040] By doping the raw coke with a binder, the isotropy of the material is improved after the binder is carbonized, the expansion is reduced, the insertion and extraction path of lithium ions during the charge and discharge process is shortened, and the fast charging performance of the material is improved.

[0041] It should be noted that in S10, the melting process needs to be performed under a protective gas atmosphere, which may be a nitrogen atmosphere, a helium atmosphere, a neon atmosphere, an argon atmosphere, or the like.

[0042] Preferably, in the present embodiment, in the operation of melting the crushed raw coke, catalyst, graphene and binder, the mass ratio of the raw coke, catalyst, graphene and binder is 100:1-5:1-5:5-15.

[0043] Preferably, in this embodiment, the binder is polyamide pitch. Polyamide pitch is mixed into the raw coke to improve the material's liquid retention performance and ion transmission path by virtue of the good isotropy, high electronic conductivity and micron-nano pores generated after carbonization of polyamide pitch.

[0044] In addition, polyamide asphalt can form an -OCO- structure and pores between graphite by relying on its own oxygen free radicals. The isotropy of polyamide asphalt formed after carbonization is high, which reduces expansion, shortens the insertion and extraction path of lithium ions during charging and discharging, and improves fast charging performance.

[0045] Specifically, in this embodiment, polyamide asphalt can be prepared by the following method: asphalt, amino acid anhydride and initiator are evenly mixed according to a mass ratio of 100:1-5:0.5-2 and stirred at a temperature of 100℃-200℃ and a speed of 500rpm-100rpm for 1h-4h, filtered and dried to obtain polyamide asphalt.

[0046] Generally speaking, the amino acid anhydride can be selected from at least one of 4-dimethylaminobenzoic anhydride, 3-dimethylaminobenzoic anhydride and 3-acetamidophthalic anhydride.

[0047] Generally speaking, the initiator can be selected from at least one of peracetic acid, peroxyacetic acid and perbenzoic acid.

[0048] Preferably, in the present embodiment, in the operation of melting the crushed raw coke, catalyst, graphene and binder, the temperature of the melting treatment is 300°C-500°C, and the time of the melting treatment is 1h-6h.

[0049] Specifically, in this embodiment, the crushed raw coke, catalyst, graphene and binder are melt-treated to obtain a mixture. The operation can be: adding the crushed raw coke, catalyst, graphene and binder to a mechanical fusion machine, heating to 300°C-500°C for melting treatment for 1h-6h, and naturally cooling to room temperature to obtain a mixture.

[0050] Preferably, in the present embodiment, in the operation of hot pressing the mixture, the hot pressing pressure is 20Mpa-50Mpa, the hot pressing time is 2h-4h, and the hot pressing temperature is 100°C-200°C.

[0051] Specifically, in this embodiment, the operation of hot pressing the mixture to obtain the graphite blocks may be: passing the mixture into a hot press, controlling the pressure to 20Mpa-50Mpa and maintaining the pressure for 2-4 hours to obtain the graphite blocks.

[0052] Preferably, in this embodiment, the raw coke is selected from at least one of petroleum coke, oil-based needle coke, coal-based needle coke and asphalt coke.

[0053] Petroleum coke is a black solid coke produced by cracking and coking vacuum residue of petroleum at 500-550℃ in a coking unit. It is generally considered to be an amorphous carbon body, or a highly aromatized high molecular carbide, a carbon body with a needle-shaped or granular structure containing tiny graphite crystals.

[0054] Petroleum coke can be used as a raw material for energy storage materials to prepare artificial graphite or porous carbon, thereby increasing the added value of petroleum coke.

[0055] Needle coke is a porous solid with a silver-grey appearance and metallic luster. It is a high-quality variety of carbon materials. Its structure has obvious flow texture, is slightly elliptical, and has a large aspect ratio. It has a fibrous or needle-like texture and feels smooth to the touch. Needle coke has the characteristics of high carbon, low sulfur, low nitrogen, and low ash. It has outstanding electrochemical and mechanical properties after graphitization. It is an anisotropic high-end carbon material that is easy to graphitize.

[0056] Needle coke can be divided into two types: oil-based needle coke and coal-based needle coke. Needle coke produced from petroleum residue is oil-based needle coke; needle coke produced from coal tar pitch and its fractions is coal-based needle coke.

[0057] Pitch coke is the solid residue obtained after high-temperature dry distillation or delayed coking of coal tar pitch. Coal tar pitch has the characteristics of abundant resources, low price, high carbon content, good fluidity, and easy graphitization. It is one of the most important and basic matrix precursors in the production of various carbon materials.

[0058] Preferably, in this embodiment, the catalyst is selected from at least one of nickel chloride, cupric chloride, ferric chloride, nickel powder, cobalt powder and iron powder.

[0059] S20, heating the compressed graphite to 500°C-800°C for pre-carbonization for 1-6h, then heating it to 2000°C-2500°C for low-temperature graphitization treatment for 6h-18h, and then heating it to 3000°C-3200°C for high-temperature graphitization treatment for 12h-48h to obtain a graphite material.

[0060] It should be noted that in S20, the operation of heat treating the graphite block needs to be performed under a protective gas atmosphere, which can be a nitrogen atmosphere, a helium atmosphere, a neon atmosphere, an argon atmosphere, etc.

[0061] The operation of adding a catalyst in S10 can accelerate the graphitization reaction process. In addition, the nanopores left by the high-temperature volatilization of the catalyst can also increase the specific surface area of ​​the material, shorten the transmission path of lithium ions during the charging and discharging process, and improve the fast charging performance of the material.

[0062] Low-temperature graphitization treatment is carried out at 2000℃-2500℃ for 6h-18h, and then the temperature is raised to 3000℃-3200℃ for high-temperature graphitization treatment; firstly, moisture, volatiles and metal impurities in the material are removed by low-temperature graphitization to improve the structural density of the material and the orientation of its carbon, and then high-temperature graphitization is carried out again to reduce the defects at the edge of the material and the regularity of its carbon rearrangement. The resulting material has the advantages of high tap density, high specific capacity and high first efficiency.

[0063] S30, heat-treating the graphite material under the condition of introducing a carbon source gas containing heteroatoms to obtain a graphite composite material.

[0064] Specifically, the prepared graphite composite material includes a core of graphite material and a shell of heteroatom-doped amorphous carbon material covering the core.

[0065] It should be noted that in S30, in order to save carbon source gas containing heteroatoms, the graphite material is heat treated under the condition of passing carbon source gas containing heteroatoms, and then cooled to room temperature under a protective gas atmosphere. The protective gas atmosphere can be a nitrogen atmosphere, a helium atmosphere, a neon atmosphere, an argon atmosphere, etc.

[0066] Preferably, in this embodiment, in the operation of heat treating the graphite material under the condition of passing a carbon source gas containing heteroatoms, the heat treatment temperature is 700°C-1000°C, the heat treatment time is 30min-300min, and the flow rate of the carbon source gas containing heteroatoms is 100ml / min-500ml / min.

[0067] Preferably, in this embodiment, the carbon source gas containing heteroatoms is at least one of CF4, COF2, CH2O, C2F4H2 and CCl3F.

[0068] It should be pointed out that the carbon source gas containing heteroatoms is the same gas, and its gas decomposition temperature is constant; however, when a mixed gas of carbon source gas and heteroatom gas is used, due to the different decomposition temperatures of the two gases, the doping uniformity of the heteroatoms and carbon atoms is poor, and the impedance reduction of the material is limited.

[0069] The preparation method of the graphite composite material of the present invention improves the compaction density of the material by doping graphene in the raw coke, relying on the high electronic conductivity and high ductility of graphene. At the same time, a catalyst is added to improve the graphitization reaction process. In addition, the nanopores left by the high-temperature volatilization of the catalyst can also increase the specific surface area of ​​the material and shorten the transmission path of lithium ions during the charging and discharging process and improve the fast charging performance of the material. At the same time, a binder is doped in the material. After the binder is carbonized, the isotropy of the material is improved, the expansion is reduced, the insertion and extraction path of lithium ions during the charging and discharging process is shortened, and the fast charging performance of the material is improved.

[0070] In addition, the preparation method of the graphite composite material of the present invention deposits heteroatom-doped amorphous carbon on the surface of the graphite material by vapor deposition. Compared with traditional liquid phase and solid phase coating methods, it has the advantages of good coating uniformity, high electronic conductivity, and reduction of the specific surface area of ​​the inner core of the prepared graphite composite material, thereby improving the fast charging performance and initial efficiency of the prepared graphite composite material.

[0071] In combination with specific embodiments, the powder conductivity and OI value of the graphite composite material prepared by the preparation method of the graphite composite material of the present invention are significantly better than those of the comparative example. The discharge specific capacity, rate and cycle performance of the negative electrode sheet prepared using this graphite composite material are significantly higher than those of the comparative example. The rate charging performance of the soft-pack battery prepared using this graphite composite material is significantly better than that of the comparative example, and the charging time is shorter, indicating that the composite negative electrode material of the present invention has good fast charging performance.

[0072] Preferably, the binder is polyamide asphalt. Polyamide asphalt is doped into the raw coke, relying on the good isotropy of polyamide asphalt, high electronic conductivity and the micron-nano pores generated after carbonization, the liquid retention performance of the material can be improved and the ion transmission path can be improved. In addition, polyamide asphalt can form -OCO- structure and pores between graphite by relying on its own oxygen free radicals, and the isotropy formed after the carbonization of polyamide asphalt is high, which reduces expansion, shortens the insertion and extraction path of lithium ions during charging and discharging, and improves fast charging performance.

[0073] The present invention also discloses a graphite composite material prepared by the above-mentioned graphite composite material preparation method in an embodiment.

[0074] Specifically, in this embodiment, the graphite composite material includes a core of graphite material and a shell of heteroatom-doped amorphous carbon material covering the core.

[0075] The graphite composite material prepared by the preparation method of the graphite composite material of the present invention improves the compaction density of the material by doping graphene in the raw coke, relying on the high electronic conductivity and high ductility of graphene. At the same time, a catalyst is added to improve the graphitization reaction process. In addition, the nanopores left by the high-temperature volatilization of the catalyst can also increase the specific surface area of ​​the material and shorten the transmission path of lithium ions during the charging and discharging process and improve the fast charging performance of the material. At the same time, a binder is doped in the material. After the binder is carbonized, the isotropy of the material is improved, the expansion is reduced, the insertion and extraction path of lithium ions during the charging and discharging process is shortened, and the fast charging performance of the material is improved.

[0076] In addition, the graphite composite material prepared by the preparation method of the graphite composite material of the present invention deposits heteroatom-doped amorphous carbon on the surface of the graphite material by vapor deposition. Compared with traditional liquid phase and solid phase coating methods, it has the advantages of good coating uniformity, high electronic conductivity, and reduction of the specific surface area of ​​the inner core of the prepared graphite composite material, thereby improving the fast charging performance and initial efficiency of the prepared graphite composite material.

[0077] In combination with specific embodiments, the powder conductivity and OI value of the graphite composite material prepared by the preparation method of the graphite composite material of the present invention are significantly better than those of the comparative example. The discharge specific capacity, rate and cycle performance of the negative electrode sheet prepared using this graphite composite material are significantly higher than those of the comparative example. The rate charging performance of the soft-pack battery prepared using this graphite composite material is significantly better than that of the comparative example, and the charging time is shorter, indicating that the composite negative electrode material of the present invention has good fast charging performance.

[0078] The invention also discloses the application of the graphite composite material in the field of energy storage devices.

[0079] For example, the graphite composite material can be applied to the field of secondary batteries.

[0080] Specifically, the graphite composite material can be used as a negative electrode material for lithium-ion secondary batteries.

[0081] In addition, the above-mentioned graphite composite materials can also be applied to fields such as supercapacitors.

[0082] The following are specific examples. In the specific examples, petroleum asphalt was purchased from Dalian Mingqiang Chemical Materials Co., Ltd., model MQ-280; coal asphalt was purchased from Hebei Fengtaiyuan Energy Technology Co., Ltd., model s001.

[0083] Example 1

[0084] A method for preparing a graphite composite material comprises the following steps:

[0085] Add 100 g of petroleum asphalt, 3 g of 4-dimethylaminobenzoic anhydride and 1 g of peracetic acid into a three-necked flask, mix well, and stir at 150° C. and 800 rpm for 2 h. Filter and vacuum dry at 80° C. for 24 h to obtain polyamide asphalt.

[0086] The petroleum coke was crushed into 10 μm and 100 g was taken, then 3 g of nickel chloride, 3 g of graphene, and 10 g of polyamide asphalt were added to a mechanical fusion machine, and heated to 400°C for melting treatment for 3 hours, and naturally cooled to room temperature to obtain a mixture; then the obtained mixture was added to a small hot press, and hot pressed at a pressure of 30 MPa and a temperature of 150°C and maintained for 3 hours to obtain a block graphite;

[0087] The compressed graphite is transferred to a graphitization furnace, heated to 650°C for pre-carbonization for 3 hours in a nitrogen atmosphere, then heated to 2200°C for low-temperature graphitization for 12 hours, then heated to 3000°C for high-temperature graphitization for 24 hours, and then cooled to graphite in a nitrogen atmosphere to obtain a graphite material;

[0088] The graphite material is transferred to a tube furnace, heated to 800°C in a nitrogen atmosphere, and CF4 gas is introduced at a flow rate of 300 ml / min for 120 minutes to obtain the desired graphite composite material. The prepared graphite composite material includes a core of the graphite material and a shell of a heteroatom-doped amorphous carbon material covering the core.

[0089] Example 2

[0090] A method for preparing a graphite composite material comprises the following steps:

[0091] 100 g of coal tar, 1 g of 3-dimethylaminobenzoic anhydride and 0.5 g of peroxyacetic acid were added to a three-necked flask, mixed evenly and stirred at 100°C at a speed of 500 rpm for 4 h, filtered, and vacuum dried at 80°C for 24 h to obtain polyamide asphalt:

[0092] The needle coke was crushed into 10 μm and 100 g was taken, then 1 g of ferric chloride, 1 g of graphene, and 5 g of polyamide asphalt were added to a mechanical fusion machine, and heated to 300°C for melting treatment for 6 hours, and naturally cooled to room temperature to obtain a mixture; then the obtained mixture was added to a small hot press, and the pressure was maintained at 20 MPa and 100°C for 4 hours to obtain a block graphite;

[0093] The compressed graphite is transferred to a graphitization furnace, heated to 500°C for pre-carbonization for 6 hours in a nitrogen atmosphere, then heated to 2000°C for low-temperature graphitization for 18 hours, then heated to 3000°C for high-temperature graphitization for 12 hours, and then cooled to graphite in a nitrogen atmosphere to obtain a graphite material;

[0094] The graphite material was transferred to a tube furnace, heated to 700°C under a nitrogen atmosphere, and COF2 gas was introduced at a flow rate of 100 ml / min for 300 min to obtain a graphite composite material. The prepared graphite composite material includes a core of the graphite material and a shell of a heteroatom-doped amorphous carbon material covering the core.

[0095] Example 3

[0096] A method for preparing a graphite composite material comprises the following steps:

[0097] 100 g of petroleum asphalt, 5 g of 3-acetylaminophthalic anhydride and 2 g of perbenzoic acid were added to a three-necked flask, mixed evenly, and stirred at 200° C. at a speed of 100 rpm for 1 h, filtered, and vacuum dried at 80° C. for 24 h to obtain polyamide asphalt;

[0098] The petroleum coke was crushed into 100g and 100g was taken, and then 5g of copper chloride, 5g of graphene and 15g of polyamide asphalt were added to a mechanical fusion machine, and heated to 500°C for melting treatment for 1h, and naturally cooled to room temperature to obtain a mixture; then the obtained mixture was added to a small hot press, and the pressure was maintained at 50Mpa and 200°C for 2h to obtain a block graphite;

[0099] The compressed graphite is transferred to a graphitization furnace, heated to 800°C for pre-carbonization for 1 hour in a nitrogen atmosphere, then heated to 2500°C for low-temperature graphitization for 6 hours, then heated to 3200°C for high-temperature graphitization for 12 hours, and then cooled to graphite in a nitrogen atmosphere to obtain a graphite material;

[0100] The graphite material is transferred to a tube furnace, heated to 1000°C in a nitrogen atmosphere, and CH2O gas is introduced at a flow rate of 500 ml / min for 30 minutes to obtain a graphite composite material. The prepared graphite composite material includes a core of the graphite material and a shell of a heteroatom-doped amorphous carbon material covering the core.

[0101] Example 4

[0102] A method for preparing a graphite composite material comprises the following steps:

[0103] Add 100 g of petroleum asphalt, 3 g of 4-dimethylaminobenzoic anhydride and 1 g of peracetic acid into a three-necked flask, mix well, and stir at 150° C. and 800 rpm for 2 h. Filter and vacuum dry at 80° C. for 24 h to obtain polyamide asphalt.

[0104] The petroleum coke was crushed into 10 μm and 100 g was taken, then 1 g of nickel chloride, 5 g of graphene, and 5 g of polyamide asphalt were added to a mechanical fusion machine, and heated to 400°C for melting treatment for 3 hours, and naturally cooled to room temperature to obtain a mixture; then the obtained mixture was added to a small hot press, and hot pressed at a pressure of 30 MPa and a temperature of 150°C and maintained for 3 hours to obtain a block graphite;

[0105] The compressed graphite is transferred to a graphitization furnace, heated to 650°C for pre-carbonization for 3 hours in a nitrogen atmosphere, then heated to 2200°C for low-temperature graphitization for 12 hours, then heated to 3000°C for high-temperature graphitization for 24 hours, and then cooled to graphite in a nitrogen atmosphere to obtain a graphite material;

[0106] The graphite material is transferred to a tube furnace, heated to 800°C in a nitrogen atmosphere, and CF4 gas is introduced at a flow rate of 300 ml / min for 120 minutes to obtain the desired graphite composite material. The prepared graphite composite material includes a core of the graphite material and a shell of a heteroatom-doped amorphous carbon material covering the core.

[0107] Example 5

[0108] A method for preparing a graphite composite material comprises the following steps:

[0109] Add 100 g of petroleum asphalt, 3 g of 4-dimethylaminobenzoic anhydride and 1 g of peracetic acid into a three-necked flask, mix well, and stir at 150° C. and 800 rpm for 2 h. Filter and vacuum dry at 80° C. for 24 h to obtain polyamide asphalt.

[0110] The petroleum coke was crushed into 10 μm and 100 g was taken, then 5 g of nickel chloride, 1 g of graphene, and 15 g of polyamide asphalt were added to a mechanical fusion machine, and heated to 400°C for melting treatment for 3 hours, and naturally cooled to room temperature to obtain a mixture; then the obtained mixture was added to a small hot press, and hot pressed at a pressure of 30 MPa and a temperature of 150°C and maintained for 3 hours to obtain a block graphite;

[0111] The compressed graphite is transferred to a graphitization furnace, heated to 650°C for pre-carbonization for 3 hours in a nitrogen atmosphere, then heated to 2200°C for low-temperature graphitization for 12 hours, then heated to 3000°C for high-temperature graphitization for 24 hours, and then cooled to graphite in a nitrogen atmosphere to obtain a graphite material;

[0112] The graphite material is transferred to a tube furnace, heated to 800°C in a nitrogen atmosphere, and CF4 gas is introduced at a flow rate of 300 ml / min for 120 minutes to obtain the desired graphite composite material. The prepared graphite composite material includes a core of the graphite material and a shell of a heteroatom-doped amorphous carbon material covering the core.

[0113] Comparative Example 1

[0114] Comparative Example 1 is substantially the same as Example 1, except that the polyamide asphalt is replaced with petroleum asphalt in Comparative Example 1.

[0115] The petroleum coke was crushed into 10 μm and 100 g was taken, then 3 g of nickel chloride, 3 g of graphene, and 10 g of petroleum asphalt were added to a mechanical fusion machine, and heated to 400°C for melting treatment for 3 hours, and naturally cooled to room temperature to obtain a mixture; then the obtained mixture was added to a small hot press, and hot pressed at a pressure of 30 MPa and a temperature of 150°C and maintained for 3 hours to obtain a block graphite;

[0116] The compressed graphite is transferred to a graphitization furnace, heated to 650°C for pre-carbonization for 3 hours in a nitrogen atmosphere, then heated to 2200°C for low-temperature graphitization for 12 hours, then heated to 3000°C for high-temperature graphitization for 24 hours, and then cooled to graphite in a nitrogen atmosphere to obtain a graphite material;

[0117] The graphite material is transferred to a tube furnace, heated to 800°C in a nitrogen atmosphere, and CF4 gas is introduced at a flow rate of 300 ml / min for 120 minutes to obtain the desired graphite composite material. The prepared graphite composite material includes a core of the graphite material and a shell of a heteroatom-doped amorphous carbon material covering the core.

[0118] Comparative Example 2

[0119] Comparative Example 2 is substantially the same as Example 1, except that nickel chloride and graphene are not added in Comparative Example 2.

[0120] Add 100 g of petroleum asphalt, 3 g of 4-dimethylaminobenzoic anhydride and 1 g of peracetic acid into a three-necked flask, mix well, and stir at 150° C. and 800 rpm for 2 h. Filter and vacuum dry at 80° C. for 24 h to obtain polyamide asphalt.

[0121] The petroleum coke was crushed into 10 μm and 100 g was taken, then 10 g of polyamide asphalt was added to a mechanical fusion machine, and heated to 400°C for melting treatment for 3 hours, and naturally cooled to room temperature to obtain a mixture; then the obtained mixture was added to a small hot press, and hot pressed at a pressure of 30 MPa and a temperature of 150°C and maintained for 3 hours to obtain a block graphite;

[0122] The compressed graphite is transferred to a graphitization furnace, heated to 650°C for pre-carbonization for 3 hours in a nitrogen atmosphere, then heated to 2200°C for low-temperature graphitization for 12 hours, then heated to 3000°C for high-temperature graphitization for 24 hours, and then cooled to graphite in a nitrogen atmosphere to obtain a graphite material;

[0123] The graphite material is transferred to a tube furnace, heated to 800°C in a nitrogen atmosphere, and CF4 gas is introduced at a flow rate of 300 ml / min for 120 minutes to obtain the desired graphite composite material. The prepared graphite composite material includes a core of the graphite material and a shell of a heteroatom-doped amorphous carbon material covering the core.

[0124] Comparative Example 3

[0125] Comparative Example 3 is substantially the same as Example 1, except that COF2 gas is not introduced into Comparative Example 3, and the rest is the same as Example 1.

[0126] Add 100 g of petroleum asphalt, 3 g of 4-dimethylaminobenzoic anhydride and 1 g of peracetic acid into a three-necked flask, mix well, and stir at 150° C. and 800 rpm for 2 h. Filter and vacuum dry at 80° C. for 24 h to obtain polyamide asphalt.

[0127] The petroleum coke was crushed into 10 μm and 100 g was taken, then 3 g of nickel chloride, 3 g of graphene, and 10 g of polyamide asphalt were added to a mechanical fusion machine, and heated to 400°C for melting treatment for 3 hours, and naturally cooled to room temperature to obtain a mixture; then the obtained mixture was added to a small hot press, and hot pressed at a pressure of 30 MPa and a temperature of 150°C and maintained for 3 hours to obtain a block graphite;

[0128] The compressed graphite is transferred to a graphitization furnace, heated to 650°C for pre-carbonization for 3 hours in a nitrogen atmosphere, then heated to 2200°C for low-temperature graphitization for 12 hours, then heated to 3000°C for high-temperature graphitization for 24 hours, and then cooled to graphite in a nitrogen atmosphere to obtain a graphite material;

[0129] The graphite material is transferred to a tube furnace and heated to 800° C. in a nitrogen atmosphere to obtain the desired graphite composite material. The prepared graphite composite material includes a core of the graphite material and a shell of an amorphous carbon material covering the core.

[0130] Test Case

[0131] (1) SEM test

[0132] The graphite composite material prepared in Example 1 was subjected to SEM testing, and the results were as follows: Figure 2 shown.

[0133] Depend on Figure 2 It can be seen that the obtained composite material presents a granular structure with slight bonding and a small amount of microporous structure on the surface. The particle size is between 10 μm and 15 μm, and the size distribution is uniform.

[0134] (2) Button battery test

[0135] The graphite composite materials prepared in Examples 1-3 and the graphite composite materials in Comparative Examples 1-3 were respectively used as negative electrode materials and assembled into button batteries according to the following methods:

[0136] Add a binder, a conductive agent, and a solvent to the negative electrode material, stir and mix them evenly to form a negative electrode slurry, apply the negative electrode slurry on a copper foil, dry, roll, and cut to obtain a negative electrode sheet. The binder is polyvinylidene fluoride, the conductive agent is SP conductive agent, the solvent is NMP, and the weight ratio of the negative electrode material, SP conductive agent, polyvinylidene fluoride and NMP is 95:1:4:220. Use a metal lithium sheet as a counter electrode, a polyethylene (PE) film, a polypropylene (PP) film or a polyethylene propylene (PEP) composite film as a separator, and LiPF6 / EC+DEC (the concentration of LiPF6 is 1.3 mol / L, and the volume ratio of EC and DEC is 1:1) as an electrolyte, and assemble the battery in an argon-filled glove box.

[0137] The button cells were installed on the Newwell CT-4008-5V10mA battery tester, and charged and discharged at a rate of 0.1C. The charge and discharge voltage range was 0.005V to 2.0V, and the first discharge capacity and first discharge efficiency were measured. The 2C rate discharge capacity was tested, and the rate performance (2C / 0.1C), cycle performance (0.1C / 0.1C, 100 weeks) and initial charge DCR (50% SOC) were calculated.

[0138] According to the national standard GB / T-24533-2019 "Graphite Anode Materials for Lithium-ion Batteries", the specific surface area, powder conductivity and powder OI value of the above-mentioned negative electrode materials were tested, and the test results are shown in Table 1.

[0139] Table 1

[0140]

[0141]

[0142] It can be seen from Table 1 that the discharge specific capacity, rate and cycle performance of the graphite composite materials prepared in Examples 1-5 are significantly higher than those in Comparative Examples 1-3; the reason may be that the isotropic properties formed by the carbonization of amino acid anhydride in the preparation process of the graphite material in the examples are high, which reduces expansion, shortens the insertion and extraction path of lithium ions during the charge and discharge process, and improves the rate performance; at the same time, heteroatom amorphous carbon is deposited on the outer layer by vapor deposition, which improves the electronic conductivity of the material, improves the powder electronic conductivity of the material, and improves the rate performance.

[0143] (3) Soft pack battery test

[0144] The graphite composite materials prepared in Examples 1-5 and the graphite composite materials in Comparative Examples 1-3 were used as negative electrode materials to prepare negative electrodes, lithium iron phosphate was used as positive electrode material to prepare positive electrodes, LiPF6 (solvent is EC+DEC, volume ratio is 1:1, concentration is 1.1 mol / L) was used as electrolyte, and celegard2400 was used as separator to prepare 2Ah soft-pack batteries.

[0145] When preparing the negative electrode, a binder, a conductive agent, and a solvent are added to the negative electrode material, stirred and mixed to form a negative electrode slurry, and the negative electrode slurry is coated on a copper foil, dried, rolled, and cut to form a negative electrode sheet. The binder is LA132 binder, the conductive agent is SP conductive agent, the solvent is double distilled water, and the weight ratio of the negative electrode material, SP conductive agent, LA132 binder and double distilled water is 95:1:4:220.

[0146] When preparing the positive electrode, a binder, a conductive agent, and a solvent are added to the positive electrode material, and the mixture is stirred and mixed to form a positive electrode slurry. The positive electrode slurry is coated on an aluminum foil, dried, rolled, and cut to form a positive electrode sheet. The binder is PVDF, the conductive agent is SP, and the solvent is N-methylpyrrolidone. The weight ratio of the positive electrode material, the conductive agent, the binder, and the solvent is 93:3:4:140.

[0147] 1) Rate performance test

[0148] The charge and discharge voltage range is 2.8V-4.2V, the test temperature is 25±3.0℃, and the charging is performed at 1.0C, 2.0C, 5.0C, and 10.0C, and the discharging is performed at 1.0C. The constant current ratio of the battery under different charging modes is tested, and the results are shown in Table 2.

[0149] Table 2

[0150] magnification 1C 2C 5C 10C Example 1 Constant current ratio (%) 96.56 91.37 82.18 63.81 Example 2 Constant current ratio (%) 95.76 90.54 80.88 60.29 Example 3 Constant current ratio (%) 97.58 93.21 84.34 67.36 Example 4 Constant current ratio (%) 97.98 93.76 85.12 69.04 Example 5 Constant current ratio (%) 95.01 89.45 79.45 65.34 Comparative Example 1 Constant current ratio (%) 90.11 83.45 68.76 51.66 Comparative Example 2 Constant current ratio (%) 92.86 85.49 72.25 55.75 Comparative Example 3 Constant current ratio (%) 92.98 86.78 74.34 59.98

[0151] From Table 2, it can be seen that the rate charging performance of the soft-pack battery using the graphite composite materials prepared in Examples 1-5 as the negative electrode material is significantly better than that of the comparative example, and the charging time is shorter, indicating that the composite negative electrode material of the present invention has good fast charging performance. The reason may be that the graphite composite materials prepared in Examples 1-5 have high powder conductivity and low OI value, which reduces expansion and improves the fast charging performance of the graphite composite materials prepared in Examples 1-5.

[0152] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a graphite composite material, characterized in that: The steps include: The crushed raw coke, catalyst, graphene and binder are melt-treated to obtain a mixture, and then the mixture is hot-pressed to obtain a briquetted graphite; The compressed graphite is heated to 500-800°C for pre-carbonization for 1-6 hours, then heated to 2000-2500°C for low-temperature graphitization for 6 hours to 18 hours, and then heated to 3000-3200°C for high-temperature graphitization for 12 hours to 48 hours to obtain a graphite material; The graphite material is heat treated under the condition of introducing carbon source gas containing heteroatoms to obtain a graphite composite material.

2. The method for preparing the graphite composite material according to claim 1, characterized in that: In the operation of melting the crushed raw coke, catalyst, graphene and binder, the mass ratio of the raw coke, the catalyst, the graphene and the binder is 100:1-5:1-5:5-15.

3. The method for preparing the graphite composite material according to claim 2, characterized in that: The binder is polyamide asphalt; The polyamide asphalt is prepared by the following method: asphalt, amino acid anhydride and initiator are mixed evenly according to a mass ratio of 100:1-5:0.5-2, stirred at a temperature of 100°C-200°C and a speed of 500rpm-100rpm for 1h-4h, filtered and dried to obtain the polyamide asphalt.

4. The method for preparing the graphite composite material according to claim 3, characterized in that: The amino acid anhydride is selected from at least one of 4-dimethylaminobenzoic anhydride, 3-dimethylaminobenzoic anhydride and 3-acetylaminophthalic anhydride; The initiator is selected from at least one of peracetic acid, peroxyacetic acid and perbenzoic acid.

5. The method for preparing the graphite composite material according to claim 2, characterized in that: In the operation of melting the crushed raw coke, catalyst, graphene and binder, the temperature of the melting treatment is 300° C.-500° C., and the time of the melting treatment is 1 h-6 h; In the operation of hot pressing the mixture, the pressure of the hot pressing is 20Mpa-50Mpa, the time of the hot pressing is 2h-4h, and the temperature of the hot pressing is 100°C-200°C.

6. The method for preparing the graphite composite material according to claim 2, characterized in that: The raw coke is selected from at least one of petroleum coke, oil-based needle coke, coal-based needle coke and asphalt coke; The catalyst is selected from at least one of nickel chloride, cupric chloride, ferric chloride, nickel powder, cobalt powder and iron powder.

7. The method for preparing a graphite composite material according to any one of claims 1 to 6, characterized in that: In the operation of heat treating the graphite material under the condition of introducing a carbon source gas containing heteroatoms, the heat treatment temperature is 700°C-1000°C, the heat treatment time is 30min-300min, and the flow rate of the carbon source gas containing heteroatoms is 100ml / min-500ml / min.

8. The method for preparing the graphite composite material according to claim 7, characterized in that: The carbon source gas containing heteroatoms is at least one of CF4, COF2, CH2O, C2F4H2 and CCl3F.

9. A graphite composite material, characterized in that: The graphite composite material is prepared by the method for preparing the graphite composite material according to any one of claims 1 to 8.

10. Use of the graphite composite material according to claim 9 in the field of energy storage devices.

Citation Information

Patent Citations

  • Preparation method of high-energy-density and fast-charging graphite negative electrode material of lithium battery

    CN114824233A

  • Method for improving softening point of asphalt through chemical grafting modification

    CN115093571A

  • Fast charging graphite and preparation method thereof, negative plate and battery

    CN116588923A

  • Non-bituminous binders made from biosourced phenolic compounds and manufacturing methods