Method for producing fumed silica by using organic silicon, polycrystalline silicon high-low-boiling-point substances and cracking kettle substrate

Through high-temperature vaporization treatment and combustion hydrolysis reaction, the high and low boiling materials of organic silicon and polycrystalline silicon and the cracking kettle substrate are converted into gas-phase silica, solving the problems of resource waste and environmental pollution, and achieving high-quality and environmentally friendly production results .

CN118954522APending Publication Date: 2024-11-15SHENYANG DONGTI FUTURE ENGINEERING TECHNOLOGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411047617.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art is difficult to effectively recycle and reuse high and low boiling materials and cracked kettle substrates generated by the silicone and polysilicon industries, resulting in waste of resources and environmental pollution.

Method used

The gas phase method mixed with hydrogen and air after high-temperature vaporization is adopted to generate silica particles through combustion hydrolysis reaction, and the vapor phase method of silica products with narrow particle size distribution and good quality are obtained by cyclone separation, deacidification and deslag treatment. .

Benefits of technology

It has achieved efficient use of by-products of the silicone and polysilicon industries to produce gas-phase silica. The product quality is excellent, the particle size distribution is narrow, and the production cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954522A_ABST
    Figure CN118954522A_ABST
Patent Text Reader

Abstract

The invention discloses a method for producing fumed silica by using organic silicon, polycrystalline silicon high-low boiling-point substances and a cracking kettle substrate, and belongs to the technical field of inorganic nano powder. The method comprises the following steps: by taking organic silicon, polycrystalline silicon high-low boiling residues and a cracking kettle substrate as raw materials, mixing gas generated after high-temperature vaporization treatment with hydrogen and air, and then putting the mixture into a hydrolysis reactor for combustion hydrolysis reaction to generate silicon dioxide particles; and carrying out cyclone separation, cloth bag separation, deacidification in a deacidification device and deslagging treatment on aggregated particles aggregated by the aggregator to obtain a finished product of the gas-phase-method silicon dioxide. The silicon dioxide product prepared by the method disclosed by the invention is narrow in particle size distribution, unimodal in distribution and good in product quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inorganic nano powders, and in particular to a method for producing gas phase silicon dioxide by utilizing organosilicon, polysilicon high and low boiling products and cracking kettle bottoms. Background Art

[0002] Fumed silica is a high-tech inorganic nano-fine chemical product. It is a silica particle generated under high temperature and high flow rate. It has a unique structure of aggregates with high specific surface area (50-400 square meters / gram), high filling and high porosity. It has reinforcing, thickening, thixotropic, matting, dispersible and insulating properties. It is widely used in many industrial fields such as rubber, coatings, adhesives, cosmetics, medicines, pesticides, inks, plastics, medicines, pesticides, sealants, colloidal batteries, polishing fluids, dry powder systems, etc., and has broad development prospects.

[0003] At present, silicone and polysilicon manufacturers produce about 300,000 tons of high and low boiling products and cracking kettle bottoms each year. Currently, they are hydrolyzed and neutralized with alkaline substances or sent to incineration devices for incineration. Therefore, how to recycle and reuse the high and low boiling products and cracking kettle bottoms produced by the silicone industry is a technical problem that my country urgently needs to solve. Summary of the invention

[0004] The object of the present invention is to provide a method for producing fumed silica by utilizing high and low boiling points of organosilicon and polysilicon and bottoms of a cracking kettle. The method utilizes by-products (high and low boiling points and bottoms of a cracking kettle) generated in the organosilicon and polysilicon industries to produce fumed silica products. The particle size distribution of the product is narrow and unimodal, and the product quality is good.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] A method for producing fumed silicon dioxide using organosilicon, high and low boiling products of polysilicon and bottoms of a cracking kettle, the method comprising the following steps:

[0007] (1) using organosilicon, polysilicon high and low boiling products and cracking kettle bottom as raw materials, mixing the gas generated after high-temperature vaporization of the raw materials with preheated hydrogen and air to obtain a mixed gas;

[0008] (2) feeding the mixed gas obtained in step (1) into a hydrolysis reactor to carry out a combustion hydrolysis reaction and generate silica particles; wherein: the reaction temperature is 1700-1800° C., the outlet temperature of the hydrolysis reactor is controlled to be 1100-1200° C., and the outlet pressure is -3-5 KPa;

[0009] (3) aggregating the reaction products after the combustion and hydrolysis reaction in step (2) into aggregated particles through an aggregator;

[0010] (4) The aggregated particles are sequentially subjected to cyclone separation, bag separation, deacidification in a deacidifier, and deslagging treatment, and then packaged by a vacuum compressor to obtain the fumed silica product.

[0011] Furthermore, in step (1), the organosilicon, polysilicon high and low boiling products and cracking kettle bottom refer to the high boiling products (high boiling point silane mixture, low boiling products (low boiling point silane mixture), high boiling kettle bottom and low boiling kettle bottom generated in the production process of organosilicon and polysilicon (the high boiling kettle bottom and the low boiling kettle bottom are the cracking kettle bottom, which is the bottom remaining in the cracking kettle after the high boiling products or low boiling products are cracked in the cracking kettle)

[0012] Furthermore, the organosilicon, polysilicon high and low boiling products and the bottom of the cracking kettle are a silane mixture with a boiling range of 26 to 215° C. and mainly composed of silicon-silicon bonds, silicon-carbon-silicon bonds, and silicon-oxygen-silicon bonds.

[0013] Furthermore, in step (1), the high-boiling substance and the high-boiling kettle bottom are subjected to high-temperature vaporization treatment using a high-boiling vaporizer, and the gas obtained after the treatment in the high-boiling vaporizer is mixed with preheated air and hydrogen and then enters a high-boiling mixer for further mixing treatment to obtain a high-boiling mixed gas; the low-boiling substance and the low-boiling kettle bottom are subjected to high-temperature vaporization treatment using a low-boiling vaporizer, and the gas generated after the treatment in the low-boiling vaporizer is mixed with preheated air and room-temperature hydrogen and then enters a low-boiling mixer for further mixing treatment to obtain a low-boiling mixed gas; after the high-boiling mixed gas and the low-boiling mixed gas are mixed together, the obtained mixed gas enters a hydrolysis reactor for treatment; the start-up of the high-boiling vaporizer and the low-boiling vaporizer are independently controlled, and can be started simultaneously or individually; valves are provided on the pipelines for conveying air and hydrogen to the high-boiling mixer and the low-boiling mixer, which can control the air and hydrogen to be conveyed to the high-boiling mixer and the low-boiling mixer at the same time, or control the air and hydrogen to be input to only one of them.

[0014] Furthermore, in step (1), the air preheating temperature is 200-300°C, and the hydrogen preheating temperature is 60-70°C;

[0015] Furthermore, in the gas entering the high-boiling mixer, the volume ratio of the hydrogen, air and the gas obtained after being treated by the high-boiling vaporizer is 1:10:0.1; in the gas entering the low-boiling mixer, the volume ratio of the hydrogen, air and the gas obtained after being treated by the low-boiling vaporizer is 1:10:0.05; wherein the hydrogen and air are both calculated based on the volume before preheating.

[0016] Furthermore, in step (1), in the high-temperature vaporization treatment, the high-boiling substances and high-boiling kettle bottom in the raw material are put into a high-boiling vaporizer for treatment, and the low-boiling substances and low-boiling kettle bottom in the raw material are put into a low-boiling vaporizer for treatment; wherein: the high-boiling vaporizer adopts a jacket and is equipped with a stirring device, 300°C heat transfer oil is introduced into the jacket of the high-boiling vaporizer, and the vaporization temperature is controlled at 220-230°C to ensure that the vaporization effect of the high-boiling substances and the high-boiling kettle bottom is uniform and stable; the low-boiling vaporizer adopts a jacket, and 0.4MPa saturated steam is introduced into the jacket, and the vaporization temperature is controlled at 70-80°C to ensure that the vaporization effect of the low-boiling substances and the low-boiling kettle bottom is uniform and stable.

[0017] Furthermore, in step (2), a raw material mixer and a burner are arranged on the top of the hydrolysis reactor, so that the flame structure can be controlled to form a relatively uniform flame state, thereby changing the residence time of the particles in the flame and the reaction temperature to control the formation and growth of the particles and obtain an ideal particle size and particle size distribution;

[0018] Furthermore, the hydrolysis reactor in step (2) and the aggregator in step (3) are both provided with a jacket, and the circulating cooling water introduced into the jacket can be high-temperature, high-pressure water above 140° C., which can generate low-pressure steam and recover waste heat to reduce costs.

[0019] Furthermore, the specific process of step (4) is as follows: the aggregated particles enter the primary cyclone separator for cyclone separation treatment, and the material output from the bottom of the primary cyclone separator enters the deacidification furnace for deacidification treatment; at the same time, the material output from the top of the primary cyclone separator enters the bag dust collector for dust removal treatment, and then is output from the bottom of the bag dust collector and returned to the primary cyclone separator for treatment; the exhaust gas discharged from the top of the bag dust collector enters the exhaust gas removal system for treatment; the material obtained after deacidification and deslagging treatment in the deacidification furnace is packaged to obtain the finished product of the fumed silica; the temperature of the deacidification treatment is 400-500°C.

[0020] Furthermore, the raw materials of the method of the present invention can also be silane compounds mainly composed of silicon-silicon bonds, silicon-carbon-silicon bonds, and silicon-oxygen-silicon bonds, such as silicon tetrachloride, trichlorosilane, and monomethyltrichlorosilane.

[0021] The advantages and beneficial effects of the present invention are as follows:

[0022] 1. The present invention inputs various reaction raw materials into the hydrolysis reactor in a certain ratio and controls the reaction gas to adopt different feed temperatures, which can ensure that the generated silica aggregates have similar size and structure, narrow particle size distribution and unimodal distribution, and good product quality.

[0023] 2. The present invention adopts a hand-combustion hydrolysis reactor with a raw material mixer and a burner on the top, which can control the flame structure and form a relatively uniform flame state, thereby changing the residence time of the particles in the flame and the reaction temperature to control the formation and growth of the particles and obtain the ideal particle size and particle size distribution.

[0024] 3. The jacket water of the hydrolysis reactor and the aggregator of the present invention adopts high-temperature and high-pressure water above 140°C, which avoids the corrosion of equipment and pipelines by hydrogen chloride condensation, prolongs the service life of equipment and pipelines, controls the impurity content of the product, and is beneficial to the formation and growth of particles.

[0025] 4. The deacidifier of the present invention uses low-temperature (400-500° C.) deacidification technology, which ensures normal deacidification of the deacidifier material while not destroying the surface chemical structure of silicon dioxide, thereby ensuring product quality.

[0026] In summary, the silica product produced by the present invention has similar aggregate size and structure, good product quality, generates flash steam, and has reasonable energy utilization. It effectively utilizes high and low boiling products in the organosilicon and polysilicon industries and the bottom of the cracking kettle to produce gas-phase silica. It is a high-tech and environmentally friendly process method for producing gas-phase silica. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a working principle diagram of the high boiling vaporizer of the present invention.

[0028] Figure 2 It is a working principle diagram of the low boiling vaporizer of the present invention.

[0029] Figure 3 The figure is a simplified flow chart of the high temperature vaporization treatment and hydrolysis reaction in the method of the present invention.

[0030] Figure 4 The present invention is a simplified flow chart of the process of agglomerated particles undergoing cyclone separation, bag separation, deacidification in a deacidifier and deslagging treatment.

[0031] Figure 5 This is the particle size distribution diagram of the silicon dioxide product prepared in Example 1. DETAILED DESCRIPTION

[0032] The present invention is further described in detail below through the accompanying drawings and embodiments.

[0033] The by-products generated in the production process of organosilicon\polysilicon in the present invention are one or more of high boiling substances (high boiling point silane mixture, low boiling substances (low boiling point silane mixture), high boiling kettle bottoms and low boiling kettle bottoms (high boiling kettle bottoms and low boiling kettle bottoms are cracking kettle bottoms, which are the bottoms remaining in the cracking kettle after the high boiling substances or low boiling substances are cracked in the cracking kettle).

[0034] The organic silicon, polysilicon high and low boiling products and cracking kettle bottom are silane mixtures with a boiling range of 26-215° C. and mainly silicon-silicon bonds, silicon-carbon-silicon bonds and silicon-oxygen-silicon bonds.

[0035] The high boiling vaporizer used in the present invention is as follows Figure 1 As shown, it adopts a jacket with a stirring device, 300°C heat transfer oil is introduced into the jacket of the high-boiling vaporizer, and the vaporization temperature is controlled at 220-230°C to ensure uniform and stable vaporization of high-boiling substances and high-boiling kettle bottoms.

[0036] The low boiling vaporizer used in the present invention is as follows Figure 2 As shown, a jacket is used, and 0.4MPa saturated steam is introduced into the jacket, and the vaporization temperature is controlled at 70-80°C to ensure uniform and stable vaporization of low-boiling substances and low-boiling kettle bottoms.

[0037] The top of the hydrolysis reactor used in the present invention is provided with a raw material mixer and a burner, which can control the flame structure and form a relatively uniform flame state, thereby changing the residence time of the particles in the flame and the reaction temperature to control the formation and growth of the particles and obtain an ideal particle size and particle size distribution;

[0038] In the present invention, the hydrolysis reactor and the aggregator are both provided with a jacket, and the circulating cooling water introduced into the jacket is high-temperature, high-pressure water above 140° C., which can generate low-pressure steam and recover waste heat to reduce costs.

[0039] The aggregator in the present invention is a conventional device, which is used to aggregate fine particles into larger particles. Its function is to change the interaction force between particles so that they aggregate into larger clusters or particles, which can remove particles and pollutants in the exhaust gas, thereby facilitating subsequent treatment or separation.

[0040] The reaction equation involved in the present invention is as follows:

[0041] CH 3 CH 3 Si 2 Cl 2 +4.5O 2 =2SiO 2 +4HCl+2CO 2 +H 2 O (1);

[0042] CH 3 CH 3 CH 3 CH 3 Si 2 Cl 2 +8.5O 2 =2SiO 2+2HCl+4CO 2 +5H 2 From (2);

[0043] CH 3 CH 3 CH 3 CH 3 CH 3 CH 3 Si 2 +11.5O 2 =2SiO 2 +6CO 2 +9H 2 From (3);

[0044] CH 3 CH 3 CH 3 Si 2 Cl 3 +6.5O 2 =2SiO 2 +3HCl+3CO 2 +3H 2 From (4);

[0045] CH 3 CH 3 CH 3 SiCl 3 +6O 2 =SiO 2 +HCl+3CO 2 +4H 2 From (5);

[0046] CH 3 CH 3 SiCl 2 +5O 2 =SiO 2 +2HCl+3CO 2 +2H 2 From (6);

[0047] CH 3 SiHCl 2 +2.5O 2 =SiO 2 +2HCl+CO 2 +H 2 From (7);

[0048] CH 3 SiCl 3 +2O 2 =SiO 2 +3HCl+CO 2 (8);

[0049] Si 2 Cl 6 +0.5O 2 +3H 2 O=2SiO 2 +6HCl (9).

[0050] Embodiment 1:

[0051] This embodiment is a method for preparing fumed silicon dioxide using by-products generated during the production of organosilicon and polysilicon as raw materials. The raw materials are high boiling substances, low boiling substances, high boiling still bottoms and low boiling still bottoms. The preparation process is as follows: Figure 3-4 , the specific preparation process is as follows:

[0052] (1) Divide the raw materials into two groups and perform high-temperature vaporization treatment separately:

[0053] The first group of raw materials are high boiling substances and high boiling substance cracking products. The high boiling substances and high boiling substance cracking products are transported to a high boiling vaporizer for high-temperature vaporization treatment at 225°C. The gas obtained after the treatment in the high boiling vaporizer is mixed with preheated air and preheated hydrogen and then enters a high boiling mixer for mixing treatment to obtain a high boiling mixed gas.

[0054] The second group of raw materials are low-boiling substances and low-boiling substance cracking products. The low-boiling substances and low-boiling substance cracking products are transported to a low-boiling vaporizer for high-temperature vaporization treatment at 75°C. The gas obtained after treatment in the low-boiling vaporizer is mixed with preheated air and room-temperature hydrogen and then enters a low-boiling mixer for mixing treatment to obtain a low-boiling mixed gas.

[0055] In this embodiment, the high-boiling vaporizer and the low-boiling vaporizer are started and operated simultaneously; the gases obtained after being treated by the high-boiling vaporizer and the low-boiling vaporizer are transmitted to the high-boiling mixer and the low-boiling mixer respectively; the air is divided into two branches after being treated by the air buffer tank, and each air branch is heated by the air heater and transmitted to the high-boiling mixer and the low-boiling mixer respectively; the hydrogen is also divided into two branches after being treated by the air buffer tank, one hydrogen branch is heated by the hydrogen heater and transmitted to the high-boiling mixer, and the other hydrogen branch is directly transmitted to the low-boiling mixer without heating.

[0056] In this embodiment, the air preheating temperature is 260°C and the hydrogen preheating temperature is 65°C.

[0057] In this embodiment, in the gas entering the high-boiling mixer, the volume ratio of the hydrogen, air and the gas obtained after being treated by the high-boiling vaporizer is 1:10:0.1; in the gas entering the low-boiling mixer, the volume ratio of the hydrogen, air and the gas obtained after being treated by the low-boiling vaporizer is 1:10:0.05; wherein the hydrogen and air are both calculated based on the volume before preheating.

[0058] (2) The high-boiling mixed gas and the low-boiling mixed gas obtained in step (1) are combined together, and the obtained mixed gas is then input into a hydrolysis reactor for combustion hydrolysis reaction to generate silica particles.

[0059] When the combustion hydrolysis reaction is carried out, the reaction temperature is 1750°C, the outlet temperature of the hydrolysis reactor is controlled to be 1160°C, and the outlet pressure is -4KPa.

[0060] (3) aggregating the reaction products after the combustion and hydrolysis reaction in step (2) into aggregated particles through an aggregator;

[0061] (4) The aggregated particles are subjected to cyclone separation, bag separation, deacidification and deslagging treatment in a deacidifier, and then packaged by a vacuum compressor to obtain the fumed silica product; the specific process of this step is as follows:

[0062] The aggregated particles enter the primary cyclone separator for cyclone separation treatment, the material output from the top of the primary cyclone separator enters the bag dust collector for dust removal treatment, and then is output from the bottom of the bag dust collector and returned to the primary cyclone separator for treatment; the exhaust gas discharged from the top of the bag dust collector enters the exhaust gas removal system for treatment; the material output from the bottom of the primary cyclone separator enters the deacidification furnace for treatment; the material obtained after deacidification and deslagging treatment in the deacidification furnace is packaged to obtain the finished product of the fumed silica; the temperature of the deacidification treatment in this embodiment is 450°C.

[0063] The particle size distribution of the fumed silica product prepared in this example is shown in FIG. Figure 5 As shown, it can be seen that it is close to the normal distribution curve, indicating that the particle size of the product has good consistency; more than 50% of the particles in the product are in the range of 260-340nm, and 90% of the particles are 300nm. The particle size distribution of the product is narrow and unimodal, and the product quality is good.

[0064] Embodiment 2:

[0065] This embodiment is a method for preparing fumed silicon dioxide using by-products produced in the production process of organosilicon and polysilicon as raw materials. The raw materials are high boiling substances and high boiling kettle bottoms. The specific preparation process is as follows:

[0066] (1) High boiling substances and high boiling substance cracking products are transported to a high boiling vaporizer for high temperature vaporization treatment at 225° C. The gas obtained after the treatment in the high boiling vaporizer is mixed with preheated air and preheated hydrogen and then enters a high boiling mixer for mixing treatment to obtain a high boiling mixed gas.

[0067] In this embodiment, only the high-boiling vaporizer is turned on, the low-boiling vaporizer is turned off, and the air transmission branch and the hydrogen transmission branch connected to the low-boiling mixer are closed (controlled by the valves on the corresponding branches). The gas obtained after treatment by the high-boiling vaporizer is transmitted to the high-boiling mixer; at the same time, the air is treated by the air buffer tank and preheated by the air heater before being transmitted to the high-boiling mixer; the hydrogen is treated by the air buffer tank and preheated by the hydrogen heater before being transmitted to the high-boiling mixer. The air preheating temperature is 240°C, and the hydrogen preheating temperature is 65°C.

[0068] In this embodiment, in the gas entering the high boiling mixer, the volume ratio of the hydrogen, air and the gas obtained after being treated by the high boiling vaporizer is 1:10:0.1; wherein the hydrogen and air are calculated based on the volume before preheating.

[0069] (2) The high-boiling mixed gas obtained in step (1) is input into a hydrolysis reactor for combustion and hydrolysis reaction to generate silicon dioxide particles.

[0070] When the combustion hydrolysis reaction is carried out, the reaction temperature is 1760°C, the outlet temperature of the hydrolysis reactor is controlled to be 1150°C, and the outlet pressure is -4KPa.

[0071] (3) aggregating the reaction products after the combustion and hydrolysis reaction in step (2) into aggregated particles through an aggregator;

[0072] (4) The aggregated particles are subjected to cyclone separation, bag separation, deacidification and deslagging treatment in a deacidifier, and then packaged by a vacuum compressor to obtain the fumed silica product; the specific process of this step is as follows:

[0073] The aggregated particles enter the primary cyclone separator for cyclone separation treatment, the material output from the top of the primary cyclone separator enters the bag dust collector for dust removal treatment, and then is output from the bottom of the bag dust collector and returned to the primary cyclone separator for treatment; the exhaust gas discharged from the top of the bag dust collector enters the exhaust gas removal system for treatment; the material output from the bottom of the primary cyclone separator enters the deacidification furnace for treatment; the material obtained after deacidification and deslagging treatment in the deacidification furnace is packaged to obtain the finished product of the fumed silica; the temperature of the deacidification treatment in this embodiment is 450°C.

[0074] The particle size of the fumed silica product prepared in this example has good consistency; more than 50% of the product has a particle size in the range of 260-340nm, and about 90% of the product has a particle size of 300nm.

[0075] The present invention is described above by way of example. It should be noted that, without departing from the core of the present invention, any simple deformation, modification or other equivalent replacement that can be made by those skilled in the art without inventive effort falls within the protection scope of the present invention.

Claims

1. A method for producing fumed silicon dioxide using organosilicon, high and low boiling products of polysilicon and bottoms of a cracking reactor, characterized in that: The method comprises the following steps: (1) using organosilicon, polysilicon high and low boiling products and cracking kettle bottom as raw materials, mixing the gas generated after high-temperature vaporization of the raw materials with preheated hydrogen and air to obtain a mixed gas; (2) feeding the mixed gas obtained in step (1) into a hydrolysis reactor to carry out a combustion hydrolysis reaction and generate silica particles; wherein: the reaction temperature is 1700-1800° C., the outlet temperature of the hydrolysis reactor is controlled to be 1100-1200° C., and the outlet pressure is -3-5 KPa; (3) aggregating the reaction products after the combustion and hydrolysis reaction in step (2) into aggregated particles through an aggregator; (4) The aggregated particles are subjected to cyclone separation, bag separation, deacidification and deslagging treatment in a deacidifier, and then packaged by a vacuum compressor to obtain the fumed silica product.

2. The method for producing fumed silicon dioxide by using organosilicon, high and low boiling products of polysilicon and bottom of cracking reactor according to claim 1, characterized in that: In step (1), the organosilicon, polysilicon high and low boiling products and cracking kettle bottom refer to the high boiling products (high boiling point silane mixture, low boiling products (low boiling point silane mixture), high boiling kettle bottom and low boiling kettle bottom (the high boiling kettle bottom and the low boiling kettle bottom are the cracking kettle bottom, which is the bottom remaining in the cracking kettle after the high boiling products or low boiling products are cracked in the cracking kettle) generated in the production process of organosilicon and polysilicon.

3. The method for producing fumed silicon dioxide by utilizing organosilicon, high and low boiling points of polysilicon and bottoms of a cracking reactor according to claim 2, characterized in that: The organic silicon, polysilicon high and low boiling products and cracking kettle bottom are silane mixtures with a boiling range of 26-215° C. and mainly silicon-silicon bonds, silicon-carbon-silicon bonds and silicon-oxygen-silicon bonds.

4. The method for producing fumed silicon dioxide by utilizing organosilicon, high and low boiling products of polysilicon and bottoms of a cracking reactor according to claim 2, characterized in that: In step (1), the high-boiling substance and the high-boiling kettle bottom are subjected to high-temperature vaporization treatment by a high-boiling vaporizer, and the gas obtained after the treatment by the high-boiling vaporizer is mixed with preheated air and preheated hydrogen and then enters a high-boiling mixer for further mixing treatment to obtain a high-boiling mixed gas; the low-boiling substance and the low-boiling kettle bottom are subjected to high-temperature vaporization treatment by a low-boiling vaporizer, and the gas generated after the treatment by the low-boiling vaporizer is mixed with preheated air and normal-temperature hydrogen and then enters a low-boiling mixer for further mixing treatment to obtain a low-boiling mixed gas; after the high-boiling mixed gas and the low-boiling mixed gas are mixed together, the obtained mixed gas enters a hydrolysis reactor for treatment; the start-up of the high-boiling vaporizer and the low-boiling vaporizer are independently controlled, and can be started simultaneously or individually; valves are provided on the pipelines for conveying air and hydrogen to the high-boiling mixer and the low-boiling mixer, which can control the air and hydrogen to be conveyed to the high-boiling mixer and the low-boiling mixer at the same time, or control the air and hydrogen to be input to only one of them.

5. The method for producing fumed silicon dioxide by utilizing organosilicon, high and low boiling products of polysilicon and bottoms of a cracking reactor according to claim 4, characterized in that: In step (1), the air preheating temperature is 200-300°C, and the hydrogen preheating temperature is 60-70°C; Among the gas entering the high-boiling mixer, the volume ratio of the hydrogen, air and the gas obtained after being treated by the high-boiling vaporizer is 1:10:0.1; among the gas entering the low-boiling mixer, the volume ratio of the hydrogen, air and the gas obtained after being treated by the low-boiling vaporizer is 1:10:0.05; wherein the hydrogen and air are calculated based on the volumes before preheating.

6. The method for producing fumed silicon dioxide by using organosilicon, high and low boiling products of polysilicon and bottom of cracking reactor according to claim 4, characterized in that: In step (1), in the high-temperature vaporization treatment, high boiling substances and high boiling kettle bottoms in the raw materials are put into a high boiling vaporizer for treatment, and low boiling substances and low boiling kettle bottoms in the raw materials are put into a low boiling vaporizer for treatment; wherein: the high boiling vaporizer adopts a jacket and is provided with a stirring device, 300° C. heat transfer oil is introduced into the jacket of the high boiling vaporizer, and the vaporization temperature is controlled at 220-230° C. to ensure that the vaporization effect of the high boiling substances and the high boiling kettle bottom is uniform and stable; the low boiling vaporizer adopts a jacket, and 0.4 MPa saturated steam is introduced into the jacket, and the vaporization temperature is controlled at 70-80° C. to ensure that the vaporization effect of the low boiling substances and the low boiling kettle bottom is uniform and stable.

7. The method for producing fumed silicon dioxide by using organosilicon, high and low boiling products of polysilicon and bottom of cracking reactor according to claim 1, characterized in that: In step (2), a raw material mixer and a burner are arranged on the top of the hydrolysis reactor, which can control the flame structure and form a relatively uniform flame state, thereby changing the residence time of the particles in the flame and the reaction temperature to control the formation and growth of the particles and obtain the ideal particle size and particle size distribution.

8. The method for producing fumed silicon dioxide by using organosilicon, high and low boiling products of polysilicon and bottom of cracking reactor according to claim 1, characterized in that: The hydrolysis reactor in step (2) and the aggregator in step (3) are both provided with a jacket. The circulating cooling water introduced into the jacket can be high-temperature, high-pressure water above 140° C., which can generate low-pressure steam and recover waste heat to reduce costs.

9. The method for producing fumed silicon dioxide by using organosilicon, high and low boiling products of polysilicon and bottom of cracking reactor according to claim 1, characterized in that: The specific process of step (4) is as follows: the aggregated particles enter the primary cyclone separator for cyclone separation treatment, and the material output from the bottom of the primary cyclone separator enters the deacidification furnace for deacidification treatment; at the same time, the material output from the top of the primary cyclone separator enters the bag dust collector for dust removal treatment, and then is output from the bottom of the bag dust collector and returned to the primary cyclone separator for treatment; The tail gas is discharged from the top of the bag filter; the material obtained after the deacidification and deslagging treatment in the deacidification furnace is packaged to obtain the finished product of the fumed silica; the temperature of the deacidification treatment is 400-500°C.

10. The method for producing fumed silicon dioxide by using organosilicon, high and low boiling products of polysilicon and bottom of cracking reactor according to claim 1, characterized in that: The raw materials of this method can also be silane compounds mainly composed of silicon-silicon bonds, silicon-carbon-silicon bonds, and silicon-oxygen-silicon bonds, such as silicon tetrachloride, trichlorosilane, and monomethyltrichlorosilane.

Citation Information

Patent Citations

  • Method for preparing high-quality silicon dioxide by vapor phase method

    CN116621185A

  • Comprehensive utilizing method for by-product in organic silicon methyl monomer production process

    CN1587040A

  • process for the preparation of finely divided oxides

    FR1007493A