Samarium bismuth titanate and preparation method and application thereof

Preparation of samarium bismuth titanate Bi4-xSmxTi3O12 by A-position doping improves the photocatalytic activity and surface area of ​​the material, solves the problem of low photocatalytic activity of pure Bi4Ti3O12, and achieves efficient photocatalytic performance and the effect of reducing the preparation temperature.

CN118954587APending Publication Date: 2024-11-15YANGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411005313.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The photocatalytic activity of pure Bi4Ti3O12 materials is low and cannot meet the actual application needs. In the process of high-temperature preparation, Bi3+ ions are prone to volatilization, resulting in a decrease in ferroelectric performance.

Method used

Bi4-xSmxTi3O12 (BSTO) of samarium titanate (Bi4-xSmxTi3O12 (BSTO) was prepared by A-position doping. The hydrothermal reaction method was used to adjust the surface activation energy and surface area of ​​the sample to improve the photocatalytic performance.

Benefits of technology

The photocatalytic degradation efficiency of the material is improved, the degradation rate reaches 95%, and the preparation temperature is reduced, providing possibilities for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954587A_ABST
    Figure CN118954587A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of oxide material preparation, in particular to samarium bismuth titanate and a preparation method and application thereof. The bismuth samarium titanate disclosed by the invention is bismuth titanate doped with A-site samarium; the general chemical formula of the samarium bismuth titanate is Bi < 4-x > Sm < x > Ti < 3 > O < 12 >, the invention also discloses a preparation method of the samarium bismuth titanate. The preparation method comprises the following specific steps: S1, dissolving bismuth nitrate pentahydrate, samarium nitrate hexahydrate and tetrabutyl titanate in dilute nitric acid to obtain a mixed solution; s2, dropwise adding a sodium hydroxide solution into the mixed solution obtained in S1 to obtain a white suspension; s3, carrying out hydrothermal reaction on the white suspension obtained in S2 in a reaction kettle; s4, after the reaction in S3 is finished, cooling to room temperature, taking out suspension liquid, and filtering, washing, drying and grinding to obtain the samarium bismuth titanate. According to the preparation method, the preparation temperature of the material is reduced, the thickness of the obtained BSTO crystal grains is extremely small, the surface area is increased, and the photocatalytic efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of oxide material preparation, and in particular to samarium bismuth titanate and a preparation method and application thereof. Background Art

[0002] Bismuth titanate Bi4Ti3O 12 (BTO) is a bismuth layered piezoelectric material, which consists of bismuth oxide layers (Bi2O2) 2+ and perovskite-like layers (Bi2Ti3O 10 ) 12- It is arranged alternately and has the advantages of low dielectric constant and good temperature stability. It has a good application prospect in the field of high temperature and high frequency. 3+ The ions are easy to volatilize and form oxygen vacancies, which causes the ferroelectric properties of the material to decrease and cannot meet the needs of practical applications. In order to improve the dielectric properties and ferroelectric properties of the material, the researchers studied the influence of Bi4Ti3O 12 Many factors affecting performance, including preparation process, substrate material selection, electrode material, annealing temperature, doping elements and doping amounts, have been extensively studied.

[0003] In addition, the study also found that BTO has a photocatalytic effect. In the layered perovskite BTO, the perovskite-like block layer is connected with (Bi2O2) along the c-axis. 2+ The layers are staggered and an internal electric field can be formed between them. The bonding angle of Ti-O-Ti is about 180°. This structure is beneficial to reduce the recombination of charge carriers and contributes to the photocatalytic oxidation of organic pollutants. However, the photocatalytic activity of pure BTO is low, and the activity of BTO needs to be improved to meet the needs of applications. Improving the photocatalytic activity of the sample is mainly achieved through the following two aspects: (1) using doping to improve the activity of the sample; (2) increasing the surface area of ​​the sample.

[0004] Therefore, it is of great significance to develop a new bismuth titanate based on A-site doping. Summary of the invention

[0005] Purpose of the invention: The technical problem to be solved by the present invention is to 12 To solve the problem of low photocatalytic properties, a method for preparing thin Bi 4-x Sm x Ti3O 12 (BSTO) powder sample method. The photocatalytic properties of the sample are improved by increasing the sample's bulk surface area.

[0006] In order to solve the above technical problems, the present invention discloses a samarium bismuth titanate (BSTO), wherein the samarium bismuth titanate is a bismuth titanate doped with samarium at the A position; the chemical formula of the samarium bismuth titanate is Bi4-x Sm x Ti3O 12 ;

[0007] Preferably, the chemical formula of the samarium bismuth titanate is Bi3SmTi3O 12 .

[0008] The present invention also provides a method for preparing BSTO, the specific steps of which are:

[0009] S1. dissolving bismuth nitrate pentahydrate, samarium nitrate hexahydrate and tetrabutyl titanate in dilute nitric acid to obtain a mixed solution;

[0010] S2. To the mixed solution obtained in S1, a sodium hydroxide solution was added dropwise to obtain a white suspension;

[0011] S3. The white suspension obtained in S2 is subjected to a hydrothermal reaction in a reactor for 45 to 50 h;

[0012] S4. After the reaction in S3 is completed, the mixture is cooled to room temperature, and the suspension is taken out, filtered, washed, dried and ground to obtain the samarium bismuth titanate.

[0013] Among them, in S1, the mass ratio of bismuth nitrate pentahydrate, samarium nitrate hexahydrate and tetrabutyl titanate is (3-4):1:(2-3); and the concentration of the dilute nitric acid is 1-3 mol / L.

[0014] Preferably, in S1, the mass ratio of bismuth nitrate pentahydrate, samarium nitrate hexahydrate and tetrabutyl titanate is 3.3:1:2.3; and the concentration of the dilute nitric acid is 2 mol / L.

[0015] Wherein, in said S2, the concentration of the sodium hydroxide solution is 4-6 mol / L.

[0016] Preferably, in S2, the concentration of the sodium hydroxide solution is 5 mol / L;

[0017] More preferably, the volume ratio of the sodium hydroxide solution to the dilute nitric acid is 1:(1-2).

[0018] Wherein, in said S3, the filling rate of the reactor is 68-72%, and the temperature of the hydrothermal reaction is 200-240°C;

[0019] Preferably, in S3, the filling rate of the reactor is 70%, and the temperature of the hydrothermal reaction is 220°C.

[0020] Wherein, in said S4, the temperature during the drying process is controlled at 60-80°C and the time is controlled at 10-15h;

[0021] Preferably, in S4, during the drying process, the temperature is controlled at 70° C. and the drying time is controlled at 12 h.

[0022] Specifically, in some embodiments of the present invention, Bi3SmTi3O is obtained by doping Sm at the A position. 12 It is also used for the photocatalytic degradation of Rhodamine B. After 90 minutes of visible light irradiation, the degradation rate of Rhodamine B is about 95%; the degradation efficiency is significantly improved compared with the undoped one.

[0023] Beneficial effects: The BSTO prepared by the present invention changes the surface activation energy of the sample by Sm doping at the A position; the BSTO grain thickness obtained by the preparation method adopted by the present invention is extremely small, the surface area is increased, and the photocatalytic efficiency is improved; the preparation method adopted by the present invention reduces the preparation temperature of the material, providing a possibility for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments, and the above and / or other advantages of the present invention will become more clear.

[0025] Figure 1 is a flow chart of sample preparation in an embodiment of the present invention;

[0026] Figure 2 is the X-ray diffraction pattern of the sample in Example 1 of the present invention;

[0027] Figure 3 is a scanning electron microscope photograph of the sample in Example 1 of the present invention;

[0028] Figure 4 is a transmission electron microscope photograph of the sample in Example 1 of the present invention;

[0029] Figure 5 This is a photocatalytic degradation diagram of the sample in Example 1 of the present invention. DETAILED DESCRIPTION

[0030] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.

[0031] Example 1: Preparation of BSTO

[0032] (1) Sample raw material preparation

[0033] Analytical pure bismuth nitrate pentahydrate (Bi(NO3)3·5H2O), samarium nitrate hexahydrate SmN3O9·6H2O, tetrabutyl titanate Ti (C4H9O4), dilute nitric acid (HNO3), and sodium hydroxide (NaOH) were selected as raw materials, and all the raw materials were products of Shanghai Chemical Reagent Company.

[0034] (2) Preparation of BSTO samples

[0035] Weigh the raw materials according to the chemical ratio (as shown in the table below). Dissolve the weighed bismuth nitrate pentahydrate (Bi(NO3)3·5H2O), samarium nitrate hexahydrate (SmN3O9·6H2O), and tetrabutyl titanate (Ti(C4H9O4)) (the amount is shown in the table below) in 36ml of dilute nitric acid (the concentration of HNO3 is 2mol / L), add 30ml of sodium hydroxide (NaOH concentration is 5mol / L) solution dropwise, stir to form a white suspension, then put it into a reactor for hydrothermal synthesis at 220℃ for 48h (the filling rate of the reactor is about 70%), cool it naturally to room temperature, take it out and wash it with alcohol and deionized water several times. Finally, put it into a drying oven and dry it at 70℃ for 12h, and grind the product after drying.

[0036] Drug Name Molecular weight Weighing <![CDATA[Bi(NO3)3·5H2O]]> 485.07 2.205g <![CDATA[SmN3O9·6H2O]]> 444.47 0.667g <![CDATA[Ti(C4H9O4)]]> 340.32 1.563g <![CDATA[HNO3]]> 63.01 5.816g NaOH 40 6.25g

[0037] Table 1 Raw materials and amounts of raw materials for BSTO sample preparation

[0038] Example 2: Characterization of BSTO

[0039] The BSTO samples prepared in Example 1 were characterized by X-ray diffraction analyzer, scanning electron microscope and transmission electron microscope. Figure 2 This is the X-ray diffraction diagram of the sample prepared in Example 1. It can be seen from the figure that the XRD spectrum of the sample is similar to the spectrum of the three-layered perovskite sample. The lattice constants a, b and c of the sample are calculated to be 0.5383nm, 0.5380nm and 3.2675nm respectively. Figure 3 and Figure 4 The SEM and TEM photos of the samples prepared in Example 1 are shown respectively. From the SEM photos of the samples, it can be clearly seen that the sample grains are complete and have good consistency. Its morphology is a typical layered and flake structure and is very thin. After measurement, its thickness direction size is 15nm to 45nm. In addition, it can be seen from the TEM photos of the samples that its grain morphology has good consistency and is very transparent, further indicating that the sample thickness direction is very thin. The thinness of the sample thickness direction virtually increases the surface area of ​​the sample, which has positive significance for its application in photocatalysis.

[0040] Example 3: Photocatalytic ability test of BSTO

[0041] The BSTO prepared in Example 1 was subjected to a photocatalytic degradation test of Rhodamine B. Figure 5 Bi3SmTi3O is obtained by doping Sm at the A site. 12 The photocatalytic degradation diagram of Rhodamine B is shown in the figure. It can be seen from the figure that after 90 minutes of visible light irradiation, the degradation rate of Rhodamine B in this embodiment is about 95%. The degradation efficiency is significantly improved compared with the undoped one.

[0042] The present invention provides samarium bismuth titanate and its preparation method and application. There are many methods and ways to implement the technical solution. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the protection scope of the present invention. All components not specified in this embodiment can be implemented by existing technologies.

Claims

1. A samarium bismuth titanate, characterized in that: The samarium bismuth titanate is bismuth titanate doped with samarium at the A position; the general chemical formula of the samarium bismuth titanate is Bi 4-x Sm x Ti3O 12 .

2. The samarium bismuth titanate according to claim 1, characterized in that The chemical formula of samarium bismuth titanate is Bi3SmTi3O 12 .

3. The method for preparing samarium bismuth titanate according to claim 1, characterized in that: The specific steps are: S1. dissolving bismuth nitrate pentahydrate, samarium nitrate hexahydrate and tetrabutyl titanate in dilute nitric acid to obtain a mixed solution; S2. To the mixed solution obtained in S1, a sodium hydroxide solution was added dropwise to obtain a white suspension; S3. The white suspension obtained in S2 is subjected to a hydrothermal reaction in a reactor for 45 to 50 h; S4. After the reaction in S3 is completed, the mixture is cooled to room temperature, and the suspension is taken out, filtered, washed, dried and ground to obtain the samarium bismuth titanate.

4. The preparation method according to claim 3, characterized in that: In the S1, the mass ratio of bismuth nitrate pentahydrate, samarium nitrate hexahydrate and tetrabutyl titanate is (3-4):1:(2-3); and the concentration of the dilute nitric acid is 1-3 mol / L.

5. The preparation method according to claim 3, characterized in that: In the S2, the concentration of the sodium hydroxide solution is 4-6 mol / L.

6. The preparation method according to claim 3, characterized in that: In S3, the filling rate of the reactor is 68-72%, and the temperature of the hydrothermal reaction is 200-240°C.

7. The preparation method according to claim 3, characterized in that: In S4, the temperature during the drying process is controlled at 60-80° C. and the time is controlled at 10-15 hours.

8. Use of the samarium bismuth titanate as claimed in claim 1 or 2 in the field of photocatalysis.