Low-temperature fast-firing slurry containing lithium tailings and ceramic bathroom high-pressure grouting product prepared from low-temperature fast-firing slurry

By introducing lithium tailings and magnesium soil into the sanitary ceramic mud, replacing potassium-sodium feldspar, and combining high-temperature sand, the low-temperature fast firing of ceramic blanks is achieved, and the difficulty of high-temperature firing and lithium tailings utilization in the existing technology is solved. The problem of this problem reduces production costs and environmental impacts, improves production efficiency and product quality.

CN118955089AActive Publication Date: 2024-11-15FOSHAN DONGPENG SANITARY WARE +4
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411042113.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

In the prior art, the mud used for sanitary ceramic grouting mainly uses potassium-sodium feldspar as flux raw material, making it difficult to achieve low temperature and rapid firing of ceramic blanks, resulting in high production costs and low efficiency, and lithium tailings are difficult to effectively utilize as industrial waste slag. , occupy land resources and pose a threat to the ecological environment.

Method used

By introducing lithium tailings, the mud raw material formula is optimized, and the potassium, sodium feldspar is replaced, and magnesium soil and high-temperature sand is combined to reduce the firing temperature, so as to achieve low-temperature rapid firing of high-pressure grouting products, and the expansion coefficient is adjusted to stabilize the firing quality .

Benefits of technology

It realizes the low temperature and rapid firing of the bathroom ceramic blank, reduces production costs and production time, improves production efficiency, meets the product shrinkage and water absorption index, and effectively utilizes industrial waste slag lithium tailings, reducing environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004972648700000081
    Figure BDA0004972648700000081
  • Figure BDA0004972648700000091
    Figure BDA0004972648700000091
Patent Text Reader

Abstract

The invention discloses a lithium-tailing-containing low-temperature fast-firing slurry, which is prepared from the following raw materials in parts by mass: 10 to 20 parts of lithium tailings, 10 to 20 parts of china clay, 10 to 20 parts of chinastone, 10 to 20 parts of kaolin, 10 to 20 parts of sericite clay, 0 to 10 parts of black clay, 0 to 5 parts of wollastonite, 0 to 5 parts of magnesian soil, 0 to 10 parts of potassium-sodium feldspar and 5 to 15 parts of high-temperature sand. The melting temperature of the high-temperature sand ranges from 1250 DEG C to 1300 DEG C. According to the low-temperature fast-firing slurry containing the lithium tailings and the ceramic bathroom high-pressure grouting product thereof provided by the technical scheme, the raw material formula of the slurry is optimized by introducing the lithium tailings, so that low-temperature fast firing of a bathroom ceramic green body is realized, the production cost of the bathroom ceramic product is greatly reduced, and the production efficiency is improved. And meanwhile, the production efficiency of bathroom ceramic products is improved, and the defects in the prior art are overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sanitary ceramics, and in particular to a low-temperature fast-burning mud containing lithium tailings and a ceramic sanitary high-pressure grouting product thereof. Background Art

[0002] Lithium tailings, as industrial waste residues generated in the production process of lithium materials, are closely related to the rapid development of the lithium materials industry. For every ton of lithium carbonate produced, eight to ten tons of lithium tailings will be produced. With the surge in market demand for lithium materials, the output of lithium tailings has also increased year by year. However, the utilization value of lithium tailings itself is low, and it is forced to be stored because it is difficult to use effectively. This treatment method not only occupies a large amount of land resources, but also poses a potential threat to the ecological environment.

[0003] According to the process, toilet bases in sanitary ceramics are generally divided into traditional grouting products and high-pressure grouting products. Both grouting products include single-sided grouting structure and double-sided grouting structure, and the double-sided grouting structure in high-pressure grouting products reaches more than 80%. Compared with the single-sided grouting structure, the double-sided grouting structure has lower requirements for the firing of the ceramic body. Therefore, ceramic sanitary products based on the high-pressure grouting process provide conditions for low-temperature fast firing of the ceramic body.

[0004] In the prior art, the slurry used for grouting of sanitary ceramics mainly uses potassium feldspar as a flux raw material. However, since potassium feldspar is a high-temperature element in the ceramic firing temperature, it is difficult to achieve low-temperature fast firing of sanitary ceramic blanks. Summary of the invention

[0005] The purpose of the present invention is to propose a low-temperature fast-firing mud containing lithium tailings and a ceramic sanitary ware high-pressure grouting product thereof. The raw material formula of the mud is optimized by introducing lithium tailings, thereby realizing low-temperature fast-firing of sanitary ware ceramic bodies, greatly reducing the production cost of sanitary ware ceramic products, and improving the production efficiency of sanitary ware ceramic products, so as to overcome the shortcomings of the prior art.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] A low-temperature fast-burning mud containing lithium tailings includes the following raw materials in parts by mass: 10-20 parts of lithium tailings, 10-20 parts of china clay, 10-20 parts of china stone, 10-20 parts of kaolin, 10-20 parts of sericite clay, 0-10 parts of black mud, 0-5 parts of wollastonite, 0-5 parts of magnesia soil, 0-10 parts of potassium-sodium feldspar and 5-15 parts of high-temperature sand;

[0008] The melting temperature of the high temperature sand is 1250-1300°.

[0009] Preferably, in terms of mass percentage, the Li2O content of the lithium tailings is 0.2-3%.

[0010] Preferably, the lithium tailings include the following chemical components in terms of mass percentage: SiO2 65-75%, Al2O3 15-25%, Fe2O3 0-0.5%, TiO2 0-0.1%, CaO 0-1%, MgO 0-1%, K2O 1-5%, Na2O 1-10% and Li2O 0.2-3%, with the remainder being loss on ignition.

[0011] Preferably, the lithium tailings include the following chemical components in mass percentage: SiO2 69.56%, Al2O3 18.7%, Fe2O3 0.48%, TiO2 0.06%, CaO 0.88%, MgO 0.21%, K2O 2.72%, Na2O 4.22% and Li2O 0.27%, and the rest is loss on ignition.

[0012] Preferably, the particle size of the lithium tailings is ≤0.6 mm.

[0013] Preferably, the magnesia soil comprises the following chemical components in percentage by mass: SiO2 62.12%, Al2O3 0.36%, Fe2O3 0.83%, TiO2 0.01%, CaO 0.42%, MgO 30.75%, K2O 0.20% and Na2O 0.12%, with the remainder being loss on ignition.

[0014] Preferably, the high temperature sand comprises the following chemical components in percentage by mass: SiO2 69.67%, Al2O3 20.04%, Fe2O3 0.76%, TiO2 0.13%, CaO 0.62%, MgO 0.02%, K2O 2.73% and Na2O 0.61%, with the remainder being loss on ignition.

[0015] Preferably, the china clay comprises the following chemical components in terms of mass percentage: SiO2 70.18%, Al2O3 18.19%, Fe2O3 0.49%, TiO2 0.01%, CaO 0.52%, MgO 0.01%, K2O 4.73% and Na2O 0.86%, with the remainder being loss on ignition;

[0016] The sericite clay material comprises the following chemical components in terms of mass percentage: SiO2 67.52%, Al2O3 22.28%, Fe2O3 0.14%, TiO2 0.02%, CaO 0.13%, MgO 0.01%, K2O 4.53% and Na2O1.23%, with the remainder being loss on ignition;

[0017] The black mud comprises the following chemical components in terms of mass percentage: SiO2 55.09%, Al2O3 27.39%, Fe2O3 1.40%, TiO2 0.05%, CaO 0.30%, MgO 0.01%, K2O 1.76% and Na2O 0.61%, with the remainder being loss on ignition.

[0018] According to the mass percentage, a low-temperature fast-burning mud containing lithium tailings includes the following raw materials: 15 parts of lithium tailings, 15 parts of porcelain clay, 15 parts of porcelain stone, 15 parts of kaolin, 15 parts of sericite clay, 10 parts of black mud, 2 parts of wollastonite, 5 parts of magnesia clay and 8 parts of high-temperature sand.

[0019] A ceramic sanitary ware high-pressure grouting product is prepared using the low-temperature fast-burning slurry containing the lithium tailings. The ceramic sanitary ware high-pressure grouting product has a firing temperature of 1215-1225° C. and a firing cycle of 14-16 hours.

[0020] The technical solution provided by the present invention may include the following beneficial effects:

[0021] 1. The introduction of industrial waste lithium tailings into the mud formula replaces the conventional high-temperature material potassium-sodium feldspar in the prior art, which can reduce the firing temperature while ensuring the fluxing effect, achieve low-temperature fast firing of high-pressure grouting products, and improve the production efficiency of sanitary ceramic products. At the same time, the shrinkage rate and water absorption rate of the fired products can meet the production indicators. Furthermore, this scheme also adds cheap magnesia clay to the mud formula to cooperate with lithium tailings, which is conducive to further reducing the firing temperature; further, due to the coordination of magnesia clay and lithium tailings, the amount of high-temperature sand added in the mud formula of this scheme is lower than that of the conventional formula, and the overall reduction of the firing temperature can be achieved by reducing the raw proportion of mullite. In addition, since lithium tailings are industrial waste slag, and magnesia clay is cheap, coupled with the reduction of high-temperature sand content, the production cost of low-temperature fast-firing mud has been greatly reduced, achieving effective cost reduction of sanitary ceramic products.

[0022] 2. In order to avoid deformation of the green body and affect the green body glaze matching of ceramic sanitary high-pressure grouting products, the addition amount of lithium tailings and magnesia clay in the low-temperature fast-firing mud is limited, so as to adjust the expansion coefficient of the mud and stabilize the firing quality of the green body. DETAILED DESCRIPTION

[0023] A low-temperature fast-burning mud containing lithium tailings, comprising the following raw materials in parts by mass: 10-20 parts of lithium tailings, 10-20 parts of china clay, 10-20 parts of china stone, 10-20 parts of kaolin, 10-20 parts of sericite clay, 0-10 parts of black mud, 0-5 parts of wollastonite, 0-5 parts of magnesia clay, 0-10 parts of potassium-sodium feldspar and 5-15 parts of high-temperature sand;

[0024] The melting temperature of the high temperature sand is 1250-1300°.

[0025] In the prior art, the slurry used for grouting of sanitary ceramics mainly uses potassium feldspar as a flux raw material. However, since potassium feldspar is a high-temperature element in the ceramic firing temperature, it is difficult to achieve low-temperature fast firing of sanitary ceramic blanks.

[0026] In order to achieve low-temperature fast firing of sanitary ceramic bodies, this technical solution proposes a low-temperature fast-firing mud suitable for ceramic sanitary high-pressure grouting products. The raw material formula of the mud is optimized by introducing lithium tailings, which is beneficial to reducing the production cost of sanitary ceramic products while improving the production efficiency of sanitary ceramic products.

[0027] Specifically, this solution introduces industrial waste lithium tailings into the mud formula to replace the conventional high-temperature material potassium-sodium feldspar in the prior art, which can reduce the firing temperature while ensuring the fluxing effect, realize low-temperature fast firing of high-pressure grouting products, and improve the production efficiency of sanitary ceramic products. At the same time, the shrinkage rate and water absorption rate of the fired products can reach the production indicators. Furthermore, this solution also adds cheap magnesia clay to the mud formula to cooperate with lithium tailings, which is conducive to further reducing the firing temperature; further, due to the coordination of magnesia clay and lithium tailings, the amount of high-temperature sand added in the mud formula of this solution is lower than that of the conventional formula, and the raw proportion of mullite can be reduced to achieve an overall decrease in the firing temperature. In addition, since lithium tailings are industrial waste, and magnesia clay is cheap, coupled with the reduction in the content of high-temperature sand, the production cost of low-temperature fast-firing mud has been greatly reduced, achieving effective cost reduction of sanitary ceramic products.

[0028] More specifically, the addition of lithium battery tailings in the formula is also beneficial to increase the grouting thickness of the product during high-pressure grouting, thereby improving the grouting efficiency by reducing the grouting time. However, in order to avoid deformation of the green body and affect the green body glaze matching of ceramic sanitary high-pressure grouting products, this solution needs to limit the addition amount of lithium tailings and magnesia clay in the low-temperature fast-firing mud, thereby adjusting the expansion coefficient of the mud to stabilize the firing quality of the green body.

[0029] To further illustrate, in terms of mass percentage, the Li2O content of the lithium tailings is 0.2-3%.

[0030] In a preferred embodiment of the present technical solution, the Li2O content of the lithium tailings is used as a material selection condition, which is more conducive to ensuring its fluxing effect.

[0031] To further illustrate, the lithium tailings include the following chemical components in terms of mass percentage: SiO2 65-75%, Al2O3 15-25%, Fe2O3 0-0.5%, TiO2 0-0.1%, CaO 0-1%, MgO 0-1%, K2O 1-5%, Na2O 1-10% and Li2O 0.2-3%, with the remainder being loss on ignition.

[0032] Further, the lithium tailings include the following chemical components in terms of mass percentage: SiO2 69.56%, Al2O3 18.7%, Fe2O3 0.48%, TiO2 0.06%, CaO 0.88%, MgO 0.21%, K2O 2.72%, Na2O4.22% and Li2O 0.27%, with the remainder being loss on ignition.

[0033] It is further stated that the particle size of the lithium tailings is ≤0.6 mm.

[0034] In another preferred embodiment of the present technical solution, the present solution also optimizes the particle size of the lithium tailings. The lithium tailings with the above particle size are easier to ball mill and have fine particles. During ball milling, the particle size distribution moves from 30 μm to 20 μm, increasing the number of larger particles in the middle and reducing the number of coarse particles, which can effectively improve the movement displacement of the particles when they are pushed by pressure during the high-pressure grouting process.

[0035] To further illustrate, the magnesia soil includes the following chemical components in terms of mass percentage: SiO2 62.12%, Al2O3 0.36%, Fe2O3 0.83%, TiO2 0.01%, CaO 0.42%, MgO 30.75%, K2O 0.20% and Na2O 0.12%, with the remainder being loss on ignition.

[0036] The MgO content of the magnesia soil added in this solution is as high as 30%, which can more effectively cooperate with the lithium tailings to achieve low-temperature rapid burning.

[0037] To further illustrate, the high temperature sand includes the following chemical components in terms of mass percentage: SiO2 69.67%, Al2O3 20.04%, Fe2O3 0.76%, TiO2 0.13%, CaO 0.62%, MgO 0.02%, K2O 2.73% and Na2O 0.61%, with the remainder being loss on ignition.

[0038] It is further stated that the china clay comprises the following chemical components in terms of mass percentage: SiO2 70.18%, Al2O3 18.19%, Fe2O3 0.49%, TiO2 0.01%, CaO 0.52%, MgO 0.01%, K2O 4.73% and Na2O0.86%, with the remainder being loss on ignition;

[0039] The sericite clay material comprises the following chemical components in terms of mass percentage: SiO2 67.52%, Al2O3 22.28%, Fe2O3 0.14%, TiO2 0.02%, CaO 0.13%, MgO 0.01%, K2O 4.53% and Na2O1.23%, with the remainder being loss on ignition;

[0040] The black mud comprises the following chemical components in terms of mass percentage: SiO2 55.09%, Al2O3 27.39%, Fe2O3 1.40%, TiO2 0.05%, CaO 0.30%, MgO 0.01%, K2O 1.76% and Na2O 0.61%, with the remainder being loss on ignition.

[0041] To further explain, the low-temperature fast-burning mud containing lithium tailings includes the following raw materials, according to the mass percentage: 15 parts of lithium tailings, 15 parts of porcelain clay, 15 parts of porcelain stone, 15 parts of kaolin, 15 parts of sericite clay, 10 parts of black mud, 2 parts of wollastonite, 5 parts of magnesia clay and 8 parts of high-temperature sand.

[0042] This technical solution also provides an optimal formula for low-temperature fast-burning mud containing lithium tailings, the slurry absorption thickness of which can reach 7.3mm / 45min, and under the firing conditions of a firing temperature of 1215-1225°C and a firing cycle of 14-16h, the shrinkage rate and water absorption rate of the green product can meet the production requirements.

[0043] A ceramic sanitary ware high-pressure grouting product is prepared using the low-temperature fast-burning slurry containing the lithium tailings. The ceramic sanitary ware high-pressure grouting product has a firing temperature of 1215-1225° C. and a firing cycle of 14-16 hours.

[0044] The use of the slurry formula of the present invention to prepare ceramic sanitary high-pressure grouting products is conducive to achieving low-temperature fast firing of sanitary ceramic blanks and improving the production efficiency of sanitary ceramic products.

[0045] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0046] Example Group

[0047] The low-temperature fast-burning mud containing lithium tailings according to the raw material formula in Table 1 was used for high-pressure grouting, and the grouting thickness of each embodiment was tested; the ceramic sanitary high-pressure grouting products were obtained by firing according to the firing conditions in Table 2, and the conventional shrinkage and water absorption tests in the sanitary ceramic field were performed on the ceramic sanitary high-pressure grouting products of each embodiment, and the results are shown in Table 3 below.

[0048] Table 1 Raw material formula of low temperature fast burning mud containing lithium tailings

[0049] Raw materials (portions) Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Lithium tailings 5 10 15 15 15 15 porcelain clay 15 15 15 15 15 15 Porcelain Stone 15 15 15 15 15 15 Kaolin 15 15 15 15 15 15 Sericite clay material 15 15 15 15 15 15 Black mud 10 10 10 10 10 10 Wollastonite 2 2 2 2 2 2 Magnesium soil 3 3 3 5 5 5 Potassium-sodium feldspar 10 5 0 0 0 0 high temperature sand 10 10 10 8 8 8

[0050] in:

[0051] In terms of mass percentage, lithium tailings include the following chemical components: SiO2 69.56%, Al2O3 18.7%, Fe2O3 0.48%, TiO2 0.06%, CaO 0.88%, MgO 0.21%, K2O 2.72%, Na2O 4.22% and Li2O 0.27%, with the rest being loss on ignition.

[0052] According to mass percentage, magnesia soil includes the following chemical components: SiO2 62.12%, Al2O3 0.36%, Fe2O30.83%, TiO2 0.01%, CaO 0.42%, MgO 30.75%, K2O 0.20% and Na2O 0.12%, and the rest is loss on ignition.

[0053] According to mass percentage, the high temperature sand includes the following chemical components: SiO2 69.67%, Al2O3 20.04%, Fe2O3 0.76%, TiO2 0.13%, CaO 0.62%, MgO 0.02%, K2O 2.73% and Na2O 0.61%, and the rest is ignition loss.

[0054] In terms of mass percentage, china clay includes the following chemical components: SiO2 70.18%, Al2O3 18.19%, Fe2O30.49%, TiO2 0.01%, CaO 0.52%, MgO 0.01%, K2O 4.73% and Na2O 0.86%, the rest being loss on ignition;

[0055] According to mass percentage, the sericite clay material includes the following chemical components: SiO2 67.52%, Al2O3 22.28%, Fe2O3 0.14%, TiO2 0.02%, CaO 0.13%, MgO 0.01%, K2O 4.53% and Na2O 1.23%, and the rest is loss on ignition;

[0056] In terms of mass percentage, the black mud includes the following chemical components: SiO2 55.09%, Al2O3 27.39%, Fe2O31.40%, TiO2 0.05%, CaO 0.30%, MgO 0.01%, K2O 1.76% and Na2O 0.61%, and the rest is loss on ignition.

[0057] Table 2 Firing conditions of low temperature fast burning slurry containing lithium tailings

[0058]

[0059] Table 3 Test items for low-temperature fast-burning mud containing lithium tailings and high-pressure grouting products for ceramic sanitary ware

[0060]

[0061] From the test results in Table 3, it can be seen that this scheme optimizes the raw material formula of the mud by introducing lithium tailings, which can effectively achieve low-temperature fast firing of sanitary ceramic bodies, greatly reduce the production cost of sanitary ceramic products, and at the same time improve the production efficiency of sanitary ceramic products to overcome the shortcomings of the prior art.

[0062] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the scope of protection of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific implementations of the present invention without paying creative labor, and these methods will fall within the scope of protection of the present invention.

Claims

1. A low-temperature fast-burning mud containing lithium tailings, characterized in that: The raw materials include the following in parts by weight: 10-20 parts of lithium tailings, 10-20 parts of porcelain clay, 10-20 parts of porcelain stone, 10-20 parts of kaolin, 10-20 parts of sericite clay, 0-10 parts of black mud, 0-5 parts of wollastonite, 0-5 parts of magnesia soil, 0-10 parts of potassium-sodium feldspar and 5-15 parts of high-temperature sand; The melting temperature of the high temperature sand is 1250-1300°.

2. The low-temperature fast-burning mud containing lithium tailings according to claim 1, characterized in that: According to mass percentage, the Li2O content of the lithium tailings is 0.2-3%.

3. The low-temperature fast-burning mud containing lithium tailings according to claim 2, characterized in that: According to mass percentage, the lithium tailings include the following chemical components: SiO2 65-75%, Al2O3 15-25%, Fe2O3 0-0.5%, TiO20-0.1%, CaO 0-1%, MgO 0-1%, K2O 1-5%, Na2O 1-10% and Li2O 0.2-3%, and the rest is ignition loss.

4. The low-temperature fast-burning mud containing lithium tailings according to claim 3, characterized in that: According to mass percentage, the lithium tailings include the following chemical components: SiO2 69.56%, Al2O3 18.7%, Fe2O3 0.48%, TiO2 0.06%, CaO 0.88%, MgO 0.21%, K2O 2.72%, Na2O 4.22% and Li2O 0.27%, and the rest is loss on ignition.

5. The low-temperature fast-burning mud containing lithium tailings according to claim 1, characterized in that: The particle size of the lithium tailings is ≤0.6 mm.

6. The low-temperature fast-burning mud containing lithium tailings according to claim 1, characterized in that: The magnesia soil comprises the following chemical components in terms of mass percentage: SiO2 62.12%, Al2O3 0.36%, Fe2O3 0.83%, TiO2 0.01%, CaO 0.42%, MgO 30.75%, K2O 0.20% and Na2O 0.12%, with the remainder being loss on ignition.

7. The low-temperature fast-burning mud containing lithium tailings according to claim 1, characterized in that: The high temperature sand comprises the following chemical components in terms of mass percentage: SiO2 69.67%, Al2O3 20.04%, Fe2O3 0.76%, TiO2 0.13%, CaO 0.62%, MgO 0.02%, K2O 2.73% and Na2O 0.61%, with the remainder being loss on ignition.

8. The low-temperature fast-burning mud containing lithium tailings according to claim 1, characterized in that: The china clay comprises the following chemical components in terms of mass percentage: SiO2 70.18%, Al2O3 18.19%, Fe2O3 0.49%, TiO2 0.01%, CaO 0.52%, MgO 0.01%, K2O 4.73% and Na2O 0.86%, with the remainder being loss on ignition; The sericite clay material comprises the following chemical components in terms of mass percentage: SiO2 67.52%, Al2O3 22.28%, Fe2O3 0.14%, TiO2 0.02%, CaO 0.13%, MgO 0.01%, K2O 4.53% and Na2O 1.23%, with the remainder being loss on ignition; The black mud comprises the following chemical components in terms of mass percentage: SiO2 55.09%, Al2O3 27.39%, Fe2O3 1.40%, TiO2 0.05%, CaO 0.30%, MgO 0.01%, K2O 1.76% and Na2O 0.61%, with the remainder being loss on ignition.

9. The low-temperature fast-burning mud containing lithium tailings according to claim 1, characterized in that: In terms of mass, the following raw materials are included: 15 parts of lithium tailings, 15 parts of porcelain clay, 15 parts of porcelain stone, 15 parts of kaolin, 15 parts of sericite clay, 10 parts of black mud, 2 parts of wollastonite, 5 parts of magnesia clay and 8 parts of high-temperature sand.

10. A ceramic sanitary ware high pressure grouting product, characterized in that: The ceramic sanitary ware high-pressure grouting product is prepared using the low-temperature fast-burning mud of the lithium-containing tailings as described in any one of claims 1 to 9, and the firing temperature of the ceramic sanitary ware high-pressure grouting product is 1215 to 1225° C., and the firing cycle is 14 to 16 hours.

Citation Information

Patent Citations

  • Method for preparing ceramic from spodumene slag instead of kaolin

    CN111423223A

  • Firing method of low-temperature fast-fired glazed tile and low-temperature fast-fired glazed tile

    CN111548138A

  • Low-temperature sintered sanitary ceramic green body and preparation method thereof

    CN113929437A

  • High-plasticity and high-water-permeability high-pressure grouting slurry and preparation method thereof

    CN115159955A

  • Ceramic green body, ceramic tile and preparation method of ceramic green body

    CN115893978A