Antifouling wear-resistant composite ceramic and preparation process thereof
Patent Information
- Application Number
- CN202411016409.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-27
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-27
AI Technical Summary
Existing ceramic products have shortcomings in terms of stain resistance and wear resistance, which is difficult to meet the performance improvement needs of daily ceramic products.
Using a combination of anti-fouling and wear-resistant composite ceramics, including sintering additives, alumina, quartz, magnesium oxide, barium sulfate, magnesium aluminum spinel, dispersant, binder and kaolin, through specific stirring , ball milling, molding, degumming and firing processes to form ceramic products with excellent mechanical strength and high wear resistance.
It achieves excellent mechanical strength and good anti-fouling performance of ceramic products, improves wear resistance, enhances the surface thickness and anti-fouling performance of ceramic particles, and improves thermal stability.
Smart Images

Figure BDA0004965829270000041 
Figure BDA0004965829270000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramics, and in particular to an anti-fouling and wear-resistant composite ceramic and a preparation process thereof. Background Art
[0002] Ceramic products have the strength of metal, rich decorative effects, good wear resistance, chemical stability, and are widely used in people's daily lives and are deeply loved by people. With the development of the economy and the improvement of people's living standards, people's performance requirements for daily-use ceramics are constantly increasing. They not only require beautiful products, but also require anti-fouling, strength, glossiness and wear resistance. Summary of the invention
[0003] In view of this, the object of the present invention is to provide an anti-fouling and wear-resistant composite ceramic and a preparation process thereof, wherein the prepared daily-use ceramic product has excellent mechanical strength, good anti-fouling performance and high wear resistance.
[0004] In order to achieve the above object, the present invention provides the following technical solutions:
[0005] An antifouling and wear-resistant composite ceramic comprises the following components in parts by weight: 20-30 parts of a sintering aid, 15-18 parts of alumina, 15-18 parts of quartz, 16-18 parts of magnesium oxide, 8-10 parts of barium sulfate, 5-8 parts of magnesium aluminum spinel, 15-18 parts of a dispersant, 15-18 parts of a binder and 15-25 parts of kaolin.
[0006] Preferably, the dispersant is sodium polyacrylate, and the binder is sodium carboxymethyl cellulose.
[0007] A preparation process of an anti-fouling and wear-resistant composite ceramic comprises the following steps:
[0008] S1: preparing sintering aid;
[0009] S2: mixing a sintering aid, alumina, quartz, magnesium oxide, barium sulfate, magnesium aluminum spinel, a dispersant, a binder and kaolin, ball milling and sieving, and continuing to stir to obtain a molding material;
[0010] S3: The molding material obtained in step S2 is molded, degummed, fired, and cooled to obtain a stain-resistant and wear-resistant composite ceramic.
[0011] Preferably, the preparation process of the sintering aid in step S1 includes:
[0012] S11: mixing 2,2'-dihydroxydiethylamine, anhydrous methanol and methyl acrylate, and reacting at 35-50°C for 4-6h to obtain a polymer monomer;
[0013] S12: Trimethylolpropane, p-toluenesulfonic acid and the polymer monomer obtained in step S11 are reacted at a constant temperature of 120-140° C. for 2-4 hours to obtain a sintering aid.
[0014] Preferably, the weight ratio of the 2,2'-dihydroxydiethylamine, anhydrous methanol and methyl acrylate is 1:6:2;
[0015] The weight ratio of the trimethylolpropane, p-toluenesulfonic acid and polymer monomer is 1:2:9.
[0016] Preferably, the process of molding the molding material in step S3 specifically includes:
[0017] The molding temperature is 150-180°C, and the molding is performed at 3-6Mpa for 20-30s;
[0018] Preferably, the process of degumming the molding material in step S3 specifically includes:
[0019] Three-stage heating degumming process: the first stage: the temperature is increased from room temperature to 250°C at a heating rate of 2°C / min; the second stage: the temperature is increased from 250°C to 500°C at a heating rate of 1°C / min; the third stage: the temperature is increased from 500°C to 600°C at a heating rate of 3°C / min.
[0020] Preferably, the process of sintering the molding material in step S3 specifically includes:
[0021] The sintering process is: heating up to 1500-1700° C. at a heating rate of 4° C. / min, and keeping the temperature for 2-3 hours.
[0022] The addition of the sintering aid of the present invention can provide lubrication between ceramic particles, reduce the friction resistance between ceramic particles in the ceramic slurry, and be filled between ceramic particles as a ceramic powder bonding phase. In addition, the sintering aid after passing through the polymer has a large number of functional groups, which can form a highly branched, topological structure and is not easy to cross-link. Therefore, it is easier to penetrate into the ceramic particles and evenly distribute to produce multi-point cross-linking, which plays a filling, bonding and coating effect, significantly increases the surface thickening rate of the ceramic particles, and increases the anti-fouling performance and wear resistance of the ceramic particles.
[0023] At the same time, the present invention heats the ceramic body at a low heating rate, and the organic matter inside the ceramic body is slowly decomposed, so that the body grains gradually increase, the internal pores slowly migrate, and the loose porous state after degreasing gradually densifies and gradually tends to be stable, avoiding excessive pores caused by the decomposition of organic matter and the occurrence of interlayer bonding, thereby further improving thermal stability and wear resistance. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. In addition, it is specifically stated that the raw materials and equipment of the present invention can be obtained from commercial sources, and no longer listed one by one. Among them, the raw materials of the present invention can be obtained from commercial sources and are well known to those skilled in the art.
[0026] Embodiment 1:
[0027] A stain-resistant and wear-resistant composite ceramic comprises the following components in parts by weight: 20 parts of a sintering aid, 15 parts of aluminum oxide, 15 parts of quartz, 16 parts of magnesium oxide, 8 parts of barium sulfate, 5 parts of magnesium aluminum spinel, 15 parts of sodium polyacrylate, 15 parts of sodium carboxymethyl cellulose and 15 parts of kaolin.
[0028] A preparation process of an anti-fouling and wear-resistant composite ceramic comprises the following steps:
[0029] S1: Preparation of sintering aid:
[0030] S11: 2,2'-dihydroxydiethylamine, anhydrous methanol and methyl acrylate were mixed in a weight ratio of 1:6:2, and reacted at 35° C. for 4 hours to obtain a polymer monomer;
[0031] S12: mixing trimethylolpropane, p-toluenesulfonic acid and the polymer monomer obtained in step S11 in a weight ratio of 1:2:9, and reacting at a constant temperature of 120° C. for 2 hours to obtain a sintering aid;
[0032] S2: mixing a sintering aid, alumina, quartz, magnesium oxide, barium sulfate, magnesium aluminum spinel, a dispersant, a binder and kaolin, ball milling and sieving, and continuing to stir to obtain a molding material;
[0033] S3: The molding material obtained in step S2 is molded at 150°C and 3Mpa for 20s, and then subjected to three-stage heating degumming, namely, the first stage: the temperature is raised from room temperature to 250°C at a heating rate of 2°C / min; the second stage: the temperature is raised from 250°C to 500°C at a heating rate of 1°C / min; the third stage: the temperature is raised from 500°C to 600°C at a heating rate of 3°C / min, and finally the temperature is raised to 1500°C at a heating rate of 4°C / min, and the sintering is completed by keeping the temperature for 2h, and then cooled to room temperature to obtain anti-fouling and wear-resistant composite ceramics.
[0034] Embodiment 2:
[0035] A stain-resistant and wear-resistant composite ceramic comprises the following components in parts by weight: 30 parts of a sintering aid, 18 parts of aluminum oxide, 18 parts of quartz, 18 parts of magnesium oxide, 10 parts of barium sulfate, 8 parts of magnesium aluminum spinel, 18 parts of sodium polyacrylate, 18 parts of sodium carboxymethyl cellulose and 25 parts of kaolin.
[0036] A preparation process of an anti-fouling and wear-resistant composite ceramic comprises the following steps:
[0037] S1: Preparation of sintering aid:
[0038] S11: mixing 2,2'-dihydroxydiethylamine, anhydrous methanol and methyl acrylate in a weight ratio of 1:6:2, and reacting at 50° C. for 6 hours to obtain a polymer monomer;
[0039] S12: mixing trimethylolpropane, p-toluenesulfonic acid and the polymer monomer obtained in step S11 in a weight ratio of 1:2:9, and reacting at a constant temperature of 140° C. for 4 hours to obtain a sintering aid;
[0040] S2: mixing a sintering aid, alumina, quartz, magnesium oxide, barium sulfate, magnesium aluminum spinel, a dispersant, a binder and kaolin, ball milling and sieving, and continuing to stir to obtain a molding material;
[0041] S3: The molding material obtained in step S2 is molded at 180°C and 6Mpa for 30s, and then subjected to three-stage heating degumming, namely, the first stage: the temperature is raised from room temperature to 250°C at a heating rate of 2°C / min; the second stage: the temperature is raised from 250°C to 500°C at a heating rate of 1°C / min; the third stage: the temperature is raised from 500°C to 600°C at a heating rate of 3°C / min, and finally the temperature is raised to 1700°C at a heating rate of 4°C / min, and the sintering is completed by keeping the temperature for 3h, and cooling to room temperature to obtain anti-fouling and wear-resistant composite ceramics. .
[0042] Embodiment 3:
[0043] A stain-resistant and wear-resistant composite ceramic comprises the following components in parts by weight: 25 parts of a sintering aid, 16 parts of aluminum oxide, 16 parts of quartz, 17 parts of magnesium oxide, 9 parts of barium sulfate, 6 parts of magnesium aluminum spinel, 16 parts of sodium polyacrylate, 16 parts of sodium carboxymethyl cellulose and 20 parts of kaolin.
[0044] A preparation process of an anti-fouling and wear-resistant composite ceramic comprises the following steps:
[0045] S1: Preparation of sintering aid:
[0046] S11: mixing 2,2'-dihydroxydiethylamine, anhydrous methanol and methyl acrylate in a weight ratio of 1:6:2, and reacting at 35-50° C. for 4-6 hours to obtain a polymer monomer;
[0047] S12: mixing trimethylolpropane, p-toluenesulfonic acid and the polymer monomer obtained in step S11 in a weight ratio of 1:2:9, and reacting at a constant temperature of 120-140° C. for 2-4 hours to obtain a sintering aid;
[0048] S2: mixing a sintering aid, alumina, quartz, magnesium oxide, barium sulfate, magnesium aluminum spinel, a dispersant, a binder and kaolin, ball milling and sieving, and continuing to stir to obtain a molding material;
[0049] S3: The molding material obtained in step S2 is molded at 150-180°C and 3-6Mpa for 20-30s, and then subjected to three-stage heating degumming, namely, the first stage: the temperature is raised from room temperature to 250°C at a heating rate of 2°C / min; the second stage: the temperature is raised from 250°C to 500°C at a heating rate of 1°C / min; the third stage: the temperature is raised from 500°C to 600°C at a heating rate of 3°C / min, and finally the temperature is raised to 1500-1700°C at a heating rate of 4°C / min, and the sintering is completed by keeping the temperature for 2-3h, and cooling to room temperature to obtain anti-fouling and wear-resistant composite ceramics.
[0050] Comparative Example 1:
[0051] The preparation process of Comparative Example 1 is basically the same as that of Example 1, except that no sintering aid is used and the degumming is performed directly, specifically:
[0052] A stain-resistant and wear-resistant composite ceramic comprises the following components in parts by weight: 15 parts of aluminum oxide, 15 parts of quartz, 16 parts of magnesium oxide, 8 parts of barium sulfate, 5 parts of magnesium aluminum spinel, 15 parts of sodium polyacrylate, 15 parts of sodium carboxymethyl cellulose and 15 parts of kaolin.
[0053] A preparation process of an anti-fouling and wear-resistant composite ceramic comprises the following steps:
[0054] S1: Alumina, quartz, magnesium oxide, barium sulfate, magnesium aluminum spinel, dispersant, binder and kaolin are mixed and ball-milled, sieved and stirred continuously to obtain a molding material;
[0055] S2: The molding material obtained in step S2 is molded at 150°C and 3Mpa for 20s, then debonded at 600°C, and finally heated to 1500°C at a heating rate of 4°C / min, kept warm for 2h to complete firing, and cooled to room temperature to obtain an anti-fouling and wear-resistant composite ceramic.
[0056] The following is a performance test of the ceramic products obtained in Examples 1 to 3 of the present invention, Comparative Example 1, and ordinary ceramic products (purchased from Shenzhen Suhui Ceramics Co., Ltd.), and the test results are shown in Table 1.
[0057] Wear resistance test: Tested in accordance with GB / T3810.6-2016.
[0058] Mechanical strength test: Tested in accordance with GB / T 4740-1999.
[0059] Anti-fouling: Apply ink drops to the surface of the product and observe whether there are any obvious traces. Table 1 Test data of Examples 1-3, commercially available ceramics and Comparative Example 1
[0060] It can be seen from the above table that Examples 1-3 have good wear resistance and antifouling ability, and also good compressive strength and fracture toughness.
[0061] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. An anti-fouling and wear-resistant composite ceramic, It is characterized in that The invention comprises the following components in parts by weight: 20-30 parts of sintering aid, 15-18 parts of aluminum oxide, 15-18 parts of quartz, 16-18 parts of magnesium oxide, 8-10 parts of barium sulfate, 5-8 parts of magnesium aluminum spinel, 15-18 parts of dispersant, 15-18 parts of binder and 15-25 parts of kaolin.
2. The antifouling and wear-resistant composite ceramic according to claim 1, It is characterized in that The dispersant is sodium polyacrylate, and the binder is sodium carboxymethyl cellulose.
3. A process for preparing the antifouling and wear-resistant composite ceramic according to claim 1, It is characterized in that The following steps are involved: S1: preparing sintering aid; S2: mixing a sintering aid, alumina, quartz, magnesium oxide, barium sulfate, magnesium aluminum spinel, a dispersant, a binder and kaolin, ball milling and sieving, and continuing to stir to obtain a molding material; S3: The molding material obtained in step S2 is molded, degummed, fired, and cooled to obtain a stain-resistant and wear-resistant composite ceramic.
4. The preparation process of the antifouling and wear-resistant composite ceramic according to claim 3, It is characterized in that The preparation process of the sintering aid in step S1 includes: S11: mixing 2,2'-dihydroxydiethylamine, anhydrous methanol and methyl acrylate, and reacting at 35-50°C for 4-6h to obtain a polymer monomer; S12: Trimethylolpropane, p-toluenesulfonic acid and the polymer monomer obtained in step S11 are reacted at a constant temperature of 120-140° C. for 2-4 hours to obtain a sintering aid.
5. The preparation process of the antifouling and wear-resistant composite ceramic according to claim 4, It is characterized in that The weight ratio of the 2,2'-dihydroxydiethylamine, anhydrous methanol and methyl acrylate is 1:6:2; The weight ratio of the trimethylolpropane, p-toluenesulfonic acid and polymer monomer is 1:2:
9.
6. The preparation process of the antifouling and wear-resistant composite ceramic according to claim 3, It is characterized in that The process of molding the molding material in step S3 specifically includes: The molding temperature is 150-180° C., and the molding is performed at 3-6 MPa for 20-30 seconds.
7. The preparation process of the antifouling and wear-resistant composite ceramic according to claim 3, It is characterized in that The process of degumming the molding material in step S3 specifically includes: Three-stage heating degumming process: the first stage: the temperature is increased from room temperature to 250°C at a heating rate of 2°C / min; the second stage: the temperature is increased from 250°C to 500°C at a heating rate of 1°C / min; the third stage: the temperature is increased from 500°C to 600°C at a heating rate of 3°C / min.
8. The preparation process of the antifouling and wear-resistant composite ceramic according to claim 3, It is characterized in that The process of sintering the molding material in step S3 specifically includes: The sintering process is: heating up to 1500-1700° C. at a heating rate of 4° C. / min, and keeping the temperature for 2-3 hours.
Citation Information
Patent Citations
Building ceramic and production method thereof
CN106082979A
Whisker reinforced aluminum oxide composite ceramic as well as preparation method and application thereof
CN110483085A
Preparation method of high-toughness and high-hardness alumina-based wear-resistant ceramic
CN111848136A
Porous ceramic for air bearing as well as preparation method and application of porous ceramic
CN113061051A
High-strength and high-glossiness domestic ceramic product and preparation method thereof
CN114685143A