Strontium titanate-based relaxor ferroelectric ceramic material with high energy storage density and efficiency and preparation of strontium titanate-based relaxor ferroelectric ceramic material
By introducing BaHfO3 components into strontium titanate-based relaxed ferroelectric ceramic materials, adjusting the crystal structure and ion disorder, the problem of insufficient energy storage density and efficiency of strontium titanate-based relaxed ferroelectric ceramic materials is solved, and the problem of insufficient energy storage density and efficiency of strontium titanate-based relaxed ferroelectric ceramic materials is achieved. The improvement of high energy storage density and efficiency is suitable for high-end, miniaturized, intelligent and integrated applications.
Patent Information
- Application Number
- CN202410894226.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-04
AI Technical Summary
The existing lead-free energy-storage ceramic materials have shortcomings in energy storage density and efficiency, which limits their development in high-end, miniaturized, intelligent and integrated applications, and the remaining electrodes of strontium titanate-based relaxation ferroelectric ceramic materials The high intensity of the purification and low breakdown field strength have led to the inadequate utilization of its application potential.
By introducing an appropriate amount of BaHfO3 components into the substrate of SrTiO3 and Bi0.5Na0.5TiO3, the crystal structure and ion disorder are adjusted, the residual polarization strength is reduced and the breakdown field strength is improved, thereby improving energy storage density and efficiency. The specific method includes chemical composition (1-x) (0.5SrTiO3-0.5Bi0.5Na0.5TiO3)-xBaHfO3, x = 0.01-0.3, and uses ball milling, drying, grinding, calcining, binder grinding, molding and sintering. Prepare ceramic materials.
While retaining high polarization strength, the energy storage density and efficiency of strontium titanate-based relaxation ferroelectric ceramics are significantly improved, with an effective energy storage density of 12.4 J/cm3, an energy storage efficiency of 91.8%, and excellent performance Environmental stability and frequency cycle stability.
Smart Images

Figure CN118955122A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of dielectric energy storage ceramic materials, and in particular relates to a strontium titanate-based relaxor ferroelectric ceramic material having high energy storage density and efficiency and a preparation method thereof. Background Art
[0002] Ferroelectric materials have the ability to store electrostatic energy due to their spontaneous polarization characteristics, and they play an increasingly important role in the field of energy storage. Lead-based ferroelectric ceramics have advantages such as high polarization strength, and have great advantages in energy storage density and its application, but the use of large amounts of lead elements will seriously harm the environment and human health, and the development of lead-free ceramic capacitors has become an inevitable trend. Lead-free energy storage ceramics often have the advantages of high power density, ultra-fast charging and discharging speed, stable matrix and strong environmental adaptability, but their low energy storage density and energy storage efficiency seriously limit the development of devices towards high-end, miniaturization, intelligence and integration.
[0003] Among lead-free energy storage ceramics, the strontium titanate system has attracted attention in the field of dielectric energy storage due to its high spontaneous polarization intensity. However, due to its large residual polarization intensity and low breakdown field strength, the energy storage efficiency and energy storage density are low, which restricts the possibility of its application. In view of this, at present, strontium titanate solid solution is mainly synthesized by doping with other chemical components, but the effects of strontium titanate solid solutions of various compositions in the existing technology are limited. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a strontium titanate-based relaxor ferroelectric ceramic material with high energy storage density and efficiency and its preparation, which reduces the residual polarization strength and improves the breakdown field strength while retaining its high polarization strength, thereby improving its energy storage density and energy storage efficiency, so that it can better meet the needs of practical applications.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] In the first aspect, the present invention provides a strontium titanate-based relaxor ferroelectric ceramic material with high energy storage density and efficiency, wherein the chemical composition is (1-x)(0.5SrTiO 3 -0.5Bi 0.5 Na 0.5 TiO 3 )-xBaHfO 3 , x = 0.01-0.3.
[0007] Preferably, x = 0.1-0.3.
[0008] In the above preferred x scheme, the electric field strength that the ceramic can withstand reaches 680 kV / cm, and its effective energy storage density under this electric field is 12.4 J / cm3 , the energy storage efficiency reaches 91.8%.
[0009] In a second aspect, the present invention provides a method for preparing a strontium titanate-based relaxor ferroelectric ceramic material having both high energy storage density and efficiency, comprising the following steps:
[0010] S1: Chemical composition of the strontium titanate-based relaxor ferroelectric ceramic material with high energy storage density and efficiency according to the first aspect (1-x) (0.5SrTiO 3 -0.5Bi 0.5 Na 0.5 TiO 3 )-xBaHfO 3 Stoichiometric ratio, weigh the raw material Bi 2 O 3 、Na 2 CO 3 、TiO 2 、SrCO 3 、BaCO 3 , HfO 2 , mixing them with anhydrous ethanol and ball milling them, followed by drying, grinding, primary calcination and cooling;
[0011] S2: Add a binder to the powder sample obtained in S1 and grind and granulate it. Then, after molding, debinding and sintering are performed in sequence.
[0012] Preferably, the ball milling time in S1 is 8-10 h, and the ball milling speed is 200-400 r / min.
[0013] Preferably, the conditions for the primary calcination in S1 include: a temperature of 800-900° C. and a time of 1-3 h.
[0014] Preferably, the binder in S2 is PVA. Further preferably, the binder is introduced in the form of a solution, and the mass concentration of PVA in the solution is 5-8 wt%. Preferably, the solvent in the binder solution is deionized water.
[0015] Preferably, the forming in S2 is tabletting, and the pressure used in the tabletting process is 5-7 Mpa.
[0016] Preferably, the debinding conditions in S2 include: temperature of 500-600° C. and time of 1-3 h.
[0017] Preferably, the sintering conditions in S2 include: temperature of 1200-1300° C. and time of 1-3 h.
[0018] The beneficial effects of the above technical solution of the present invention are as follows:
[0019] By using SrTiO with a specific ratio 3 with Bi 0.5 Na 0.5 TiO 3 Into a specific substrate, an appropriate amount of BaHfO is introduced 3 , which can reduce the residual polarization strength and increase the breakdown field strength while retaining its high polarization strength, thereby improving its energy storage density and efficiency, so that it can better meet the needs of practical applications. The main reason is that the appropriate amount of BaHfO 3 Ba in the components 2+ Because of the A-site ion (Sr 2+ 、Bi 3+ 、Na + ) have appropriate differences in chemical valence or size, Hf 4+ With B-site ions (i.e. Ti 4+ ) have appropriate differences in size, and the large ionic radius of Ba 2+ It can increase the disorder of A-site ions, which is beneficial to transform the ordered macroscopic ferroelectric domains into disordered nanodomain clusters, reduce polarization hysteresis and thus improve energy storage efficiency; and with a specific ratio of SrTiO 3 with Bi 0.5 Na 0.5 TiO 3 , which can appropriately enhance the disorder of the A-site ions in the matrix crystal, further facilitating the Ba 2+ The doping solid solution increases the degree of ion disorder and thus reduces its polarization hysteresis. At the same time, the grain size of this component is small and the sample resistance is large, so that its breakdown field strength is improved, thereby improving the effective energy storage density and energy storage efficiency. Among them, the value range of x is appropriate, which is conducive to the reasonable control of the doping amount, maintaining the lattice stability while increasing the ion disorder, so that the material system composition is near the relaxation phase to obtain high energy storage performance. If x is too large, it will cause serious lattice distortion, and the system composition will deviate from the relaxation phase and fail to achieve the purpose of improving energy storage performance.
[0020] The preparation method of the present invention can obtain strontium titanate-based relaxor ferroelectric ceramics with high energy storage density and efficiency, wherein 0.7 (0.5 SrTiO 3 -0.5Bi 0.5 Na 0.5 TiO 3 )-0.3BaHfO 3 Relaxor ferroelectric ceramics, in one embodiment, have a breakdown field strength of up to 680 kV / cm, which is higher than most strontium titanate-based energy storage ceramics, and have an effective energy storage density of 12.4 J / cm 3 , the energy storage efficiency is 91.8%.
[0021] In addition, the strontium titanate-based relaxor ferroelectric ceramics of the present invention also exhibit excellent environmental stability, with an effective energy storage density of 5.35 ± 0.3 J / cm at 40-150°C. 3 ; Under 1-100 Hz test conditions, the effective energy storage density is 5.54 ± 0.05 J / cm 3 ; in 10 1 -10 8 The effective energy storage density is 5.58 ± 0.03 J / cm 3 . BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 XRD patterns of strontium titanate-based relaxor ferroelectric ceramics prepared in Comparative Example 1 and Examples 1-3;
[0023] Figure 2 is a SEM image of the strontium titanate-based relaxor ferroelectric ceramic prepared in Example 1;
[0024] Figure 3 1 is the unipolar PE curve of the strontium titanate-based relaxor ferroelectric ceramic prepared in Example 1 under different electric field strengths;
[0025] Figure 4 The curve showing the change of energy storage characteristics of the strontium titanate-based relaxor ferroelectric ceramic obtained in Example 1 with the electric field strength;
[0026] Figure 5 1 is the unipolar PE curve of the strontium titanate-based relaxor ferroelectric ceramic prepared in Example 1 at a temperature gradient of 40-150°C;
[0027] Figure 6 1 is a single-pole PE curve of the strontium titanate-based relaxor ferroelectric ceramic prepared in Example 1 at a test frequency of 1-100 Hz;
[0028] Figure 7 The strontium titanate-based relaxor ferroelectric ceramic prepared in Example 1 was heated to 10 1 -10 8 Unipolar PE curves under cycle number. DETAILED DESCRIPTION
[0029] In order to make the technical problems, technical solutions and advantages to be solved by the present invention clearer, the following will be described in detail with reference to the accompanying drawings and specific embodiments. In the following examples, the PVA binder meets the following requirements: it is introduced in the form of a solution, the solvent is deionized water, and the mass concentration of PVA in the solution is 5 wt%.
[0030] Comparative Example 1:
[0031] Preparation of 0.5SrTiO by the present invention 3-0.5Bi 0.5 Na 0.5 TiO 3 Ferroelectric ceramics. According to the chemical dosage ratio, weigh 5.8833 g Bi 2 O 3 , 1.3275 g Na 2 CO 3 , 8.1500 g TiO 2 , 7.4561 g SrCO 3 , the weighing error is between ± 0.0005 grams. Pour the weighed raw materials into the ball mill, add anhydrous ethanol and ball mill for 10 hours at a speed of 300 r / min, and dry and grind the ball-milled samples in turn. Then place the evenly mixed powder in a crucible, cover it, and put it into a muffle furnace and set the temperature to 830 ℃ for calcination for 2 hours. After cooling, take the sample and place it in a mortar, add an appropriate amount of PVA binder to grind and granulate, grind evenly, pour it into a mold of φ = 10 mm and press it into a sheet with a cold isostatic press, then put the sheet into a muffle furnace for debinding and sintering in turn, the debinding conditions are 550℃, 2h, and the sintering conditions are 1220℃, 2h, and strontium titanate ferroelectric ceramic material can be obtained. After cooling, the ceramic sheet is polished to a thickness of 40-50 μm, and gold-plated electrodes are sprayed on its upper and lower surfaces for energy storage performance testing (the same is true for subsequent examples of energy storage performance testing).
[0032] In this example, the maximum electric field strength that can be applied is 80 kV / cm, at which point the total energy storage density is 1.97 J / cm 3 , effective energy storage density reaches 0.59 J / cm 3 , the energy storage efficiency reaches 29.9%.
[0033] Embodiment 1:
[0034] The present invention is used to prepare 0.7 (0.5SrTiO 3 -0.5Bi 0.5 Na 0.5 TiO 3 )-0.3BaHfO 3 Ferroelectric ceramics. According to the chemical dosage ratio, weigh 4.1183 g of Bi 2 O 3 , 0.9293 g Na 2 CO 3 , 5.7050 g TiO 2 , 5.2192 g SrCO 3 , 5.9800 g BaCO 3 , 6.4436 g HfO 2, the weighing error is between ± 0.0005 grams. Pour the weighed raw materials into a ball mill, add anhydrous ethanol and ball mill for 10 hours at a speed of 300 r / min. The ball-milled samples are dried and ground in turn. Then the mixed powder is placed in a crucible with a cover, and placed in a muffle furnace and calcined at 830 °C for 2 hours. After cooling, take the sample and place it in a mortar, add an appropriate amount of PVA binder and grind it into granules. Grind it evenly, pour it into a mold with a diameter of φ = 10 mm and press it into a sheet with a cold isostatic press. Then put the sheet into a muffle furnace for debinding and sintering in turn. The debinding conditions are 550 °C and 2 hours, and the sintering conditions are 1220 °C and 2 hours. A strontium titanate-based relaxor ferroelectric ceramic material with high energy storage density, efficiency and excellent environmental stability can be obtained.
[0035] Embodiment 2:
[0036] The method is carried out in accordance with Example 1, except that the method of preparing 0.9 (0.5 SrTiO 3 -0.5Bi 0.5 Na 0.5 TiO 3 )-0.1BaHfO 3 Ferroelectric ceramics. According to the chemical dosage ratio, weigh 5.2950 g Bi 2 O 3 , 1.1948 g Na 2 CO 3 , 7.3350 g TiO 2 , 6.7105 g SrCO 3 , 1.9933 g BaCO 3 , 2.148 g HfO 2 , the weighing error is between ± 0.0005 grams.
[0037] In this example, the maximum electric field strength that can be applied is 360 kV / cm, and the total energy storage density is 5.81 J / cm 3 , effective energy storage density reaches 3.27 J / cm 3 , the energy storage efficiency is as high as 56.3%.
[0038] Embodiment 3:
[0039] The method is carried out in accordance with Example 1, except that the 0.8 (0.5 SrTiO 3 -0.5Bi 0.5 Na 0.5 TiO 3 )-0.2BaHfO 3 Ferroelectric ceramics. Weigh 4.7066 g Bi according to the chemical dosage ratio 2 O 3, 1.0620 g Na 2 CO 3 , 6.5200 g TiO 2 , 5.9648 g SrCO 3 , 3.9867 g BaCO 3 , 4.2957 g HfO 2 , the weighing error is between ±0.0005 grams.
[0040] In this example, the maximum electric field strength that can be applied is 96 kV / cm, and the total energy storage density is 0.83 J / cm 3 , effective energy storage density reaches 0.69 J / cm 3 , the energy storage efficiency is as high as 83.1%.
[0041] Figure 1 The XRD patterns of the strontium titanate-based relaxor ferroelectric ceramic powders prepared in Comparative Example 1 and Examples 1-3 are shown in the figure. It can be seen that the prepared series of strontium titanate-based relaxor ferroelectric ceramic samples all have a single cubic perovskite structure without obvious impurity phase, indicating that BaHfO 3 The new component has been successfully dissolved into the crystal lattice of the matrix, forming a uniform solid solution.
[0042] Figure 2 This is a SEM image of the strontium titanate-based relaxor ferroelectric ceramic prepared in Example 1. It can be seen from the image that the ceramic grain size is about 1.21 μm and the density is relatively high, which is beneficial to improving the breakdown field strength of the sample.
[0043] Figure 3 The unipolar hysteresis loops of the 40-50 μm thick strontium titanate-based relaxor ferroelectric ceramics prepared in Example 1 under different electric fields. It can be seen from the figure that the ceramic hysteresis loops are slender, indicating that their remanent polarization is small, and the saturation polarization intensity gradually increases, and the maximum electric field strength can reach 680 kV / cm.
[0044] Figure 4 The energy storage characteristics of the strontium titanate-based relaxor ferroelectric ceramic obtained in Example 1 vary with the electric field strength. It can be seen that the maximum applied electric field strength is 680 kV / cm, at which time the total energy storage density is 13.6 J / cm 3 , effective energy storage density reaches 12.4 J / cm 3 , the energy storage efficiency is as high as 91.8%.
[0045] Comparative Example 2:
[0046] The method is carried out in accordance with Example 1, except that 0.7 (0.3 SrTiO 3 -0.7Bi 0.5 Na0.5 TiO 3 )-0.3BaHfO 3 Ferroelectric ceramics. Weigh 2.5945 g Bi according to the chemical dosage ratio 2 O 3 , 0.5945 g Na 2 CO 3 , 2.5412 g TiO 2 , 1.4092 g SrCO 3 , 2.6910 g BaCO 3 , 2.8703 g HfO 2 , the weighing error is between ±0.0005 grams.
[0047] In this example, the maximum electric field strength that can be applied is 65 kV / cm, and the total energy storage density is 0.88 J / cm 3 , effective energy storage density reaches 0.65 J / cm 3 , the energy storage efficiency reaches 73.6%.
[0048] Test Case
[0049] Taking Example 1 as an example, the environmental stability of the obtained product was tested.
[0050] Figure 5 The unipolar hysteresis loop of the 40-50 μm thick strontium titanate-based relaxor ferroelectric ceramic sample prepared in Example 1 under a temperature gradient of 40-150 °C. The test electric field is 400 kV / cm. Under this test condition, its effective energy storage density is 5.35± 0.3 J / cm 3 , it can be seen that the effective energy storage density of the sample is temperature stable.
[0051] Figure 6 The unipolar hysteresis loops of the 40-50 μm thick strontium titanate-based relaxor ferroelectric ceramic sample prepared in Example 1 were measured at different test frequencies at room temperature and 400 kV / cm electric field strength. The test frequency was 1-100 Hz. Under this test condition, its effective energy storage density was 5.54 ± 0.05 J / cm 3 , it can be seen that the effective energy storage density of the sample has good frequency stability.
[0052] Figure 7 The unipolar hysteresis loops of the 40-50 μm thick strontium titanate-based relaxor ferroelectric ceramic sample prepared in Example 1 were measured at different cycle numbers at room temperature and an electric field strength of 400 kV / cm. The cycle number was 10 1 -10 8 Under this test condition, its effective energy storage density is 5.58 ± 0.03 J / cm 3It can be seen that the energy storage density of the material sample has good cycle stability.
[0053] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A strontium titanate-based relaxor ferroelectric ceramic material having both high energy storage density and efficiency, characterized in that: Its chemical composition is (1-x)(0.5SrTiO3-0.5Bi 0.5 Na 0.5 TiO3)-xBaHfO3, x = 0.01-0.
3.
2. The strontium titanate-based relaxor ferroelectric ceramic material with high energy storage density and efficiency according to claim 1, characterized in that: x = 0.1-0.3。 3. A method for preparing a strontium titanate-based relaxor ferroelectric ceramic material having both high energy storage density and efficiency, characterized in that: The steps include: S1: The chemical composition (1-x) (0.5SrTiO3-0.5Bi) of the strontium titanate-based relaxor ferroelectric ceramic material having high energy storage density and efficiency as claimed in claim 1 or 2 0.5 Na 0.5 The raw materials Bi2O3, Na2CO3, TiO2, SrCO3, BaCO3 and HfO2 are weighed, mixed with anhydrous ethanol and ball-milled, and then dried, ground, calcined once and cooled; S2: Add a binder to the powder sample obtained in S1 and grind and granulate it. Then, after molding, debinding and sintering are performed in sequence.
4. The method for preparing the strontium titanate-based relaxor ferroelectric ceramic material having both high energy storage density and efficiency according to claim 3, characterized in that: The ball milling time in S1 is 8-10 h, and the ball milling speed is 200-400 r / min.
5. The method for preparing the strontium titanate-based relaxor ferroelectric ceramic material having both high energy storage density and efficiency according to claim 3, characterized in that: The conditions for the primary calcination in S1 include: a temperature of 800-900°C and a time of 1-3 h.
6. The method for preparing the strontium titanate-based relaxor ferroelectric ceramic material with high energy storage density and efficiency according to claim 3, characterized in that: The binder in S2 is PVA, which is introduced in the form of a solution, and the mass concentration of PVA in the solution is 5-8 wt%.
7. The method for preparing the strontium titanate-based relaxor ferroelectric ceramic material having high energy storage density and efficiency according to claim 3, characterized in that: The tablets are formed in S2, and the pressure used in the tableting process is 5-7 MPa.
8. The method for preparing a strontium titanate-based relaxor ferroelectric ceramic material having high energy storage density and efficiency according to claim 3, characterized in that: The debinding conditions in S2 include: temperature of 500-600°C and time of 1-3h.
9. The method for preparing a strontium titanate-based relaxor ferroelectric ceramic material having high energy storage density and efficiency according to claim 3, characterized in that: The sintering conditions in S2 include: temperature of 1200-1300°C and time of 1-3h.
Citation Information
Patent Citations
High-energy-storage sodium bismuth titanate-strontium titanate matrix material and preparation method thereof
CN109574656A
Sodium bismuth titanate-based relaxor ferroelectric ceramic material with high energy storage density, high power density and high efficiency and preparation method of sodium bismuth titanate-based relaxor ferroelectric ceramic material
CN115196960A
Sodium bismuth titanate-based relaxor ferroelectric ceramic material with excellent energy storage performance and environmental stability and preparation method of sodium bismuth titanate-based relaxor ferroelectric ceramic material
CN116444265A
Sodium bismuth titanate-strontium titanate high-energy-storage lead-free ceramic material and preparation method thereof
CN116675529A
Composite Bismuth-based lead-free piezoelectric ceramics and process for preparing the same