Magnesium fluoride target material and preparation method thereof
Magnesium fluoride targets are prepared by two-stage heating and vacuum hot pressing, which solves the problem of difficult preparation of high-density and high-hardness magnesium fluoride targets in the prior art, and achieves the improvement of high-density and hardness performance, simplifying the The preparation process was carried out.
Patent Information
- Application Number
- CN202411284768.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art is difficult to prepare high density and high hardness magnesium fluoride targets, and the preparation method is complex, making it difficult to meet the needs of material research and preparation.
Two-stage heating and vacuum heat pressing method are used, first heated at 400~500℃ for 30~60 minutes, then heated to 850~930℃ for 50~60MPa, and cooled after releasing the pressure to obtain fluorine with high relative density and hardness. Magnesium-deficient target.
The high density and hardness performance of magnesium fluoride targets are achieved, the density and hardness performance of the targets are ensured, and the preparation process is simple and the stability is high.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the field of sputtering target material preparation, and more specifically, relates to a magnesium fluoride target material and a preparation method thereof. Background Art
[0002] Magnesium fluoride target is a material used for thin film deposition and material research. It can also be used for research and preparation in the fields of optical thin films, solar cells, semiconductor devices, etc. Magnesium fluoride target usually has high purity, uniform composition and good mechanical properties, which can meet the needs of different research and preparation.
[0003] The patent with publication number CN106587940A discloses a high-purity dense magnesium oxide target and a preparation method thereof. The method performs cold isostatic pressing on the magnesium oxide powder milled by planetary ball milling and then vacuum sintering to obtain a near-net-shaped high-purity dense magnesium oxide target. The vacuum sintering temperature is 1400~1550℃ and the holding time is 2~10h. The density of the high-purity dense magnesium oxide target prepared by this method can reach 98.36%. However, the above method is not suitable for the preparation of high-density and high-hardness magnesium fluoride targets. Summary of the invention
[0004] In view of the above problems existing in the prior art, the object of the present invention is to provide a magnesium fluoride target material and a preparation method thereof. The method is simple to operate, and the prepared magnesium fluoride target material has higher relative density and hardness index.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is: A method for preparing a magnesium fluoride target comprises the following steps: (1) Pre-pressing a mold filled with magnesium fluoride powder; (2) The mold containing magnesium fluoride powder after pre-pressing is subjected to first-stage heating and second-stage heating in sequence under vacuum conditions: the temperature of the first-stage heating is 400-500°C, and the duration of the first-stage heating is 30-60 minutes; the temperature of the second-stage heating is 850-930°C, and the duration of the second-stage heating is 45-60 minutes; wherein, pressurization is started after 5-10 minutes of the second-stage heating, and the pressurization pressure is 50-60 MPa, and the pressure is released after the second-stage heating is completed; (3) Cool the mold, take out the magnesium fluoride target blank, and obtain the magnesium fluoride target after processing.
[0006] Preferably, in step (1), the D50 of the magnesium fluoride powder is 300-600 nm.
[0007] Preferably, in step (1), the D90 of the magnesium fluoride powder is 800-950 nm.
[0008] Preferably, in step (1), the pre-pressing pressure is 30-40 MPa.
[0009] Preferably, in step (1), the duration of the pre-pressing is 5 to 10 minutes.
[0010] Preferably, in step (2), the heating rate is 5-10°C / min.
[0011] Preferably, in step (2), the second-stage heating temperature rise rate is 5-10°C / min.
[0012] Preferably, step (1) and step (2) are carried out in a vacuum hot pressing furnace.
[0013] Preferably, in step (2), the vacuum condition is an absolute vacuum degree ≤ 10Pa.
[0014] The invention also discloses a magnesium fluoride target material prepared by the preparation method.
[0015] Compared with the prior art, the present invention has the following beneficial effects: The preparation method of the magnesium fluoride target material of the present invention adopts two-stage heating to ensure uniform heating during the preparation of the target material blank. Pressurization is performed during the two-stage heating process to ensure the density and hardness performance during the preparation of the target material. The target material finally prepared has high density, high hardness and stable quality. DETAILED DESCRIPTION
[0016] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and carefully in combination with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.
[0017] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0018] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0019] Example 1 This embodiment provides a method for preparing a magnesium fluoride target, comprising the following steps: (1) Loading: evenly load magnesium fluoride powder of a certain specification into the mold. The specifications of the magnesium fluoride powder are: D50 is 600nm, D90 is 950nm; (2) Prepressing: Place the mold containing magnesium fluoride powder in a vacuum hot press furnace for prepressing at a prepressing pressure of 35 MPa for 5 min. (3) Hot pressing: Turn on the vacuum system. When the absolute vacuum degree is ≤10Pa, start the first and second stage heating. The heating rate of the first stage is 6℃ / min, and the temperature is raised to 500℃ and kept for 30min. The heating rate of the second stage is 10℃ / min, and the temperature is raised to 930℃ and kept for 45min. After the second stage heating is kept for 5min, pressurization is started. The pressurization pressure is 50MPa. Pressurization is continued until the heating is completed, and then the pressure is released. (4) Demolding: Cool the mold, take out the magnesium fluoride target blank, and obtain the magnesium fluoride target after processing.
[0020] Example 2 This embodiment provides a method for preparing a magnesium fluoride target, comprising the following steps: (1) Loading: evenly load magnesium fluoride powder of a certain specification into the mold. The specifications of the magnesium fluoride powder are: D50 is 300nm, D90 is 800nm; (2) Prepressing: Place the mold containing magnesium fluoride powder in a vacuum hot press furnace for prepressing at a prepressing pressure of 40 MPa for 6 min; (3) Hot pressing: Turn on the vacuum system. When the absolute vacuum degree is ≤10Pa, start the first and second stage heating. The heating rate of the first stage is 5℃ / min, and the temperature is raised to 400℃ and kept for 60min. The heating rate of the second stage is 5℃ / min, and the temperature is raised to 850℃ and kept for 60min. After the second stage heating is kept for 5min, start pressurization. The pressurization pressure is 55MPa. Pressurize until the heating is completed, and then release the pressure. (4) Demolding: Cool the mold, take out the magnesium fluoride target blank, and obtain the magnesium fluoride target after processing.
[0021] Example 3 This embodiment provides a method for preparing a magnesium fluoride target, comprising the following steps: (1) Loading: evenly load magnesium fluoride powder of a certain specification into the mold. The specifications of the magnesium fluoride powder are: D50 is 500nm, D90 is 950nm; (2) Prepressing: Place the mold containing magnesium fluoride powder in a vacuum hot press furnace for prepressing at a prepressing pressure of 30 MPa for 8 min. (3) Hot pressing: Turn on the vacuum system. When the absolute vacuum degree is ≤10Pa, start the first and second stage heating. The heating rate of the first stage is 10℃ / min, and the temperature is raised to 500℃ and kept for 35min. The heating rate of the second stage is 6℃ / min, and the temperature is raised to 850℃ and kept for 50min. After the second stage heating is kept for 5min, start pressurization. The pressurization pressure is 60MPa. Pressurize until the heating is completed, and then release the pressure. (4) Demolding: Cool the mold, take out the magnesium fluoride target blank, and obtain the magnesium fluoride target after processing.
[0022] Example 4 This embodiment provides a method for preparing a magnesium fluoride target, comprising the following steps: (1) Loading: evenly load magnesium fluoride powder of a certain specification into the mold. The specifications of the magnesium fluoride powder are: D50 is 500nm, D90 is 950nm; (2) Prepressing: Place the mold containing magnesium fluoride powder in a vacuum hot press furnace for prepressing at a prepressing pressure of 30 MPa for 8 min. (3) Hot pressing: Turn on the vacuum system. When the absolute vacuum degree is ≤10Pa, start the first and second stage heating. The heating rate of the first stage is 10℃ / min, and the temperature is raised to 500℃ and kept for 35min. The heating rate of the second stage is 6℃ / min, and the temperature is raised to 870℃ and kept for 50min. After the second stage heating is kept for 8min, start pressurization. The pressurization pressure is 60MPa. Pressurize until the heating is completed, and then release the pressure. (4) Demolding: Cool the mold, take out the magnesium fluoride target blank, and obtain the magnesium fluoride target after processing.
[0023] Comparative Example 1 This comparative example provides a method for preparing a magnesium fluoride target, comprising the following steps: (1) Loading: evenly load magnesium fluoride powder of a certain specification into the mold. The specifications of the magnesium fluoride powder are: D50 is 600nm, D90 is 950nm; (2) Prepressing: Place the mold containing magnesium fluoride powder in a vacuum hot press furnace for prepressing at a prepressing pressure of 35 MPa for 5 min. (3) Hot pressing: Turn on the vacuum system. When the absolute vacuum degree is ≤10Pa, start the first and second stage heating. The heating rate of the first stage is 6℃ / min, and the temperature is raised to 500℃ and kept for 30min. The heating rate of the second stage is 10℃ / min, and the temperature is raised to 950℃ and kept for 45min. After the second stage heating is kept for 5min, start pressurization. The pressurization pressure is 40MPa. Pressurize until the heating is completed, and then release the pressure. (4) Demolding: Cool the mold, take out the magnesium fluoride target blank, and obtain the magnesium fluoride target after processing.
[0024] Comparative Example 2 This comparative example provides a method for preparing a magnesium fluoride target, comprising the following steps: (1) Loading: evenly load magnesium fluoride powder of a certain specification into the mold. The specifications of the magnesium fluoride powder are: D50 is 300nm, D90 is 800nm; (2) Prepressing: Place the mold containing magnesium fluoride powder in a vacuum hot press furnace for prepressing at a prepressing pressure of 40 MPa for 6 min; (3) Hot pressing: Turn on the vacuum system. When the absolute vacuum degree is ≤10Pa, start the first and second stage heating. The heating rate of the first stage is 5℃ / min, and the temperature is raised to 400℃ and kept for 60min. The heating rate of the second stage is 5℃ / min, and the temperature is raised to 800℃ and kept for 60min. After the second stage heating is kept for 5min, start pressurization. The pressurization pressure is 55MPa. Pressurize until the heating is completed, and then release the pressure. (4) Demolding: Cool the mold, take out the magnesium fluoride target blank, and obtain the magnesium fluoride target after processing.
[0025] Comparative Example 3 This comparative example is basically the same as Example 1, except that: (3) Hot pressing: Turn on the vacuum system. When the absolute vacuum degree is ≤10Pa, start the first and second stage heating. The heating rate of the first stage is 6℃ / min, and the temperature is raised to 500℃ and kept for 30min. The heating rate of the second stage is 10℃ / min, and the temperature is raised to 930℃ and kept for 90min. After the second stage heating is kept for 15min, pressurization is started. The pressurization pressure is 50MPa. Pressurization is continued until the heating is completed, and then the pressure is released.
[0026] Comparative Example 4 This comparative example is basically the same as Example 1, except that: (3) Hot pressing: Turn on the vacuum system. When the absolute vacuum degree is ≤10Pa, start the first and second stage heating. The heating rate of the first stage is 6℃ / min, and the temperature is raised to 500℃ and kept for 30min. The heating rate of the second stage is 10℃ / min, and the temperature is raised to 980℃ and kept for 45min. After the second stage heating is kept for 5min, pressurization is started. The pressurization pressure is 50MPa. Pressurization is continued until the heating is completed, and then the pressure is released.
[0027] The relative density and hardness of the magnesium fluoride targets obtained in Examples 1 to 4 and Comparative Examples 1 to 4 were tested, and the data are shown in Table 1. It can be seen that the magnesium fluoride target prepared by the preparation method of the present invention, especially when the parameter setting is controlled within the temperature and insulation time range of the second stage heating of the present application, has a higher relative density and hardness.
[0028] Table 1 The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the scope of the present invention.
Claims
1. A method for preparing a magnesium fluoride target, characterized in that: The following steps are involved: (1) Pre-pressing a mold filled with magnesium fluoride powder; (2) The mold containing magnesium fluoride powder after pre-pressing is subjected to first-stage heating and second-stage heating in sequence under vacuum conditions: the temperature of the first-stage heating is 400-500°C, and the duration of the first-stage heating is 30-60 minutes; the temperature of the second-stage heating is 850-930°C, and the duration of the second-stage heating is 45-60 minutes; wherein, pressurization is started after 5-10 minutes of the second-stage heating, and the pressurization pressure is 50-60 MPa, and the pressure is released after the second-stage heating is completed; (3) Cool the mold, take out the magnesium fluoride target blank, and obtain the magnesium fluoride target after processing.
2. The method for preparing a magnesium fluoride target according to claim 1, characterized in that: In step (1), the D50 of the magnesium fluoride powder is 300-600 nm.
3. The method for preparing a magnesium fluoride target according to claim 1 or 2, characterized in that: In step (1), the D90 of the magnesium fluoride powder is 800-950 nm.
4. The method for preparing a magnesium fluoride target according to claim 1, characterized in that: In step (1), the pre-pressing pressure is 30-40 MPa; and the pre-pressing time is 5-10 min.
5. The method for preparing a magnesium fluoride target according to claim 1, characterized in that: In step (2), the heating rate of the first stage is 5-10°C / min.
6. The method for preparing a magnesium fluoride target according to claim 1, characterized in that: In step (2), the heating rate of the second stage heating is 5-10°C / min.
7. The method for preparing a magnesium fluoride target according to claim 1, characterized in that: Step (1) and step (2) are carried out in a vacuum hot pressing furnace.
8. The method for preparing a magnesium fluoride target according to claim 1, characterized in that: In step (2), the vacuum condition is an absolute vacuum degree ≤ 10Pa.
9. A magnesium fluoride target prepared by the preparation method according to any one of claims 1 to 8.
Citation Information
Patent Citations
Fluoride sintered compact for neutron moderator, and method for producing said fluoride sintered compact
CN104640824A
Method of preparing nanoscale magnesium fluoride transparent ceramic through hot pressing method
CN110981484A
MgF2 SYSTEM FLUORIDE SINTERED BODY FOR RADIATION MODERATOR AND METHOD FOR PRODUCING THE SAME
US20160351282A1
Fluoride sputtering target and method for preparation thereof
WO2003023084A1
Cited By
Pretreatment method of cobalt target blank for diffusion welding
CN119589103A
Preparation method of magnesium fluoride ceramic sputtering target material
CN121202565A
A method for preparing a magnesium fluoride ceramic sputtering target
CN121202565B