Acidolysis phosphate tailing particles as well as preparation method and application thereof

By slag acid activates phosphorus tailings and adds cellulose, the problem of difficult pelletization and disintegration of phosphorus tailings particles is solved, and efficient preparation of medium-element fertilizers is achieved, which meets national standards and reduces production costs.

CN118955204AInactive Publication Date: 2024-11-15CHINA AGRI UNIV

Patent Information

Application Number
CN202411023638.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Phosphorus tailings are difficult to disintegrate due to the excessive viscosity of the acid mixture, and the powder is not suitable for agricultural mechanization requirements, making it difficult to granulate, and calcium and magnesium nutrients are difficult to decompose and utilize in the soil, resulting in poor fertilizer efficiency.

Method used

By reacting slag acid as a phosphorus tailings activator with phosphorus tailings, calcium carbonate and magnesium carbonate are decomposed into calcium oxide and magnesium oxide, increasing the pore channel and specific surface area, and adding cellulose as an auxiliary agent to improve the viscosity of the granulation system and Dispersant acts to promote granulation and rapid disintegration.

Benefits of technology

It has achieved high particle strength and rapid dissolution of phosphorus tailings particles, comply with the national standard of calcium, magnesium, phosphorus fertilizer, reduced production costs, simple process, and has broad industrialization potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955204A_ABST
    Figure CN118955204A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of fertilizer preparation, and provides acidolysis phosphate tailing particles as well as a preparation method and application thereof. Comprising the following steps: mixing treated phosphate tailings and an activating agent to form a mixture, and performing an activation reaction to obtain acidolysis phosphate tailings; the acidolysis phosphate tailings and cellulose are mixed for granulation, and acidolysis phosphate tailings particles are obtained. According to the method, the sludge acid and the phosphate tailings are subjected to decomposition reaction, meanwhile, a large number of pore channels are formed on the surfaces of the phosphate tailings due to acidolysis reaction, the specific surface area of the phosphate tailings is increased, water can permeate into the phosphate tailings more easily to form a liquid bridge due to the fact that ionic bonds are damaged, and granulation is promoted while nutrients of the phosphate tailings are activated due to precipitation of magnesium ions; cellulose is added as an auxiliary agent, the viscosity of a granulation system is improved, granulation is promoted, the cellulose can serve as a dispersing agent in a particle product, the cellulose is rapidly swelled when encountering water, the phosphate tailing particles can be rapidly disintegrated, and the problem that the particle product is difficult to disintegrate due to the fact that the viscosity of a phosphate tailing acid mixture is too high is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fertilizer preparation, and in particular relates to acid-hydrolyzed phosphate tailing particles and a preparation method and application thereof. Background Art

[0002] With the continuous expansion of the scale of the phosphorus chemical industry, the accumulation of phosphorus tailings has continued to increase. At present, the annual output of phosphorus tailings has reached 700wt, but its utilization rate is only 20%. As industrial waste, phosphorus tailings are currently mainly stored in reservoirs. The construction and maintenance of tailings reservoirs are extremely expensive, and a large amount of manpower, material resources and financial resources are spent every year to ensure the safety of production and ecological environment in the tailings reservoir area. This is because most tailings are by-products of phosphorus rock after sulfuric acid acid hydrolysis. When washed by rainwater, a large amount of highly acidic water will flow to nearby land and farmland, destroying the ecological balance. In addition, some organic mineral processing agents remain in the tailings. Discharging them into the surrounding environment will cause serious pollution to the atmosphere and water and soil, and lead to water and soil depletion, plant death, and even directly threaten the living environment of humans and animals. Regardless of the treatment method, a large amount of farmland and forest land will be occupied, which will also have a serious impact on the surrounding ecological environment. How to achieve large-scale and high-value utilization of phosphorus tailings has become a current research hotspot.

[0003] 87% of the phosphorus tailings are dolomite, and its main chemical composition is calcium carbonate and magnesium carbonate, which makes it have the potential to prepare soil conditioners and medium-element fertilizers. However, powdered phosphorus tailings are not suitable for the requirements of agricultural mechanization, and many inconveniences are caused during transportation and use due to problems such as easy agglomeration and dust. However, phosphorus tailings are difficult to granulate as a typical sandy material. The higher lattice energy between calcium and magnesium ions gives its internal structure a strong electrostatic attraction, and due to the hexagonal crystal structure, the overall strength of the ionic bond is large, and the hydration energy is difficult to overcome the lattice energy, resulting in phosphorus tailings being difficult to dissolve in water and having extremely low viscosity, making it difficult to form liquid bridges during the granulation process, and thus difficult to granulate. In addition, the calcium and magnesium nutrients in phosphorus tailings exist in the form of carbonates, which are difficult to decompose and utilize in the soil, resulting in poor fertilizer efficiency. How to activate these medium elements in phosphorus tailings and prepare them into granular products has become a bottleneck technology that limits the full utilization of phosphorus chemical by-products.

[0004] Application No. 201810687284.4 discloses a granular medium-trace element fertilizer and a production method thereof, which mainly uses raw materials such as polyacrylamide, polyvinyl alcohol, lignin, etc. as binders to achieve efficient granulation of sandy materials such as yellow phosphorus slag. Although it has both high particle strength and fast disintegration rate, the binders used are mostly artificial synthetic polymers, which not only cause high production costs, but also these materials will produce microplastic pollution when applied to the soil with the fertilizer; Application No. CN202310538455.8 discloses a preparation method of low-energy calcium-magnesium phosphate fertilizer, which reacts waste phosphoric acid with phosphate tailings by acid hydrolysis, matures and crushes them, and then reacts with exogenous nutrients such as calcium oxide to obtain phosphate tailings granular products. Although good fertilizer effect has been achieved on macadamia nut crops, the invention does not disclose a detailed granulation scheme. In addition, it is not clear whether the physical properties of the final product can achieve high particle strength and rapid dissolution. Based on this, how to develop a phosphate tailings particle with simple process, low cost, high particle strength and fast dissolution for use as a fertilizer for medium and trace nutrients has become a difficult problem that urgently needs to be solved. Summary of the invention

[0005] The object of the present invention is to provide an acid-hydrolyzed phosphate tailings particle and a preparation method and application thereof, so as to solve the problem that the particle product is difficult to disintegrate due to the high viscosity of the phosphate tailings slag acid mixture. The slag acid is used as a phosphate tailings activator to react with the phosphate tailings, and calcium carbonate and magnesium carbonate are decomposed into the form of calcium oxide and magnesium oxide. At the same time, due to the acid hydrolysis reaction, carbonate ions are converted into carbon dioxide, so that a large number of pore channels are formed on the surface of the phosphate tailings, thereby increasing its specific surface area. Since the ionic bonds are destroyed, water is more likely to penetrate into the interior of the phosphate tailings to form a liquid bridge. In addition, due to the precipitation of magnesium ions, the mixture composed of the phosphate tailings and the slag acid has a high viscosity, which promotes granulation while activating the nutrients of the phosphate tailings; adding cellulose as an auxiliary agent can improve the viscosity of the granulation system and promote granulation on the one hand, and can act as a dispersant in the final particle product on the other hand. The cellulose swells rapidly in water, so that the phosphate tailings particles can be quickly disintegrated, avoiding the problem that the particle product is difficult to disintegrate due to the high viscosity of the phosphate tailings slag acid mixture.

[0006] In order to achieve the above purpose, the technical solution adopted in this application is:

[0007] The first object of the present invention is to provide a method for preparing acid-hydrolyzed phosphate tailing particles, comprising the following steps:

[0008] The treated phosphate tailings and an activator are mixed to form a mixture, and an activation reaction is performed. The activation reaction promotes the decomposition of the phosphate tailings, increases the void channels of the phosphate tailings, forms a liquid bridge, and obtains an acid-decomposed phosphate tailings;

[0009] The acid-hydrolyzed phosphate tailings and cellulose are mixed for granulation. During the granulation process, the cellulose increases the viscosity of the granulation system, promotes granulation and increases the disintegration of the phosphate tailings particles, thereby obtaining the acid-hydrolyzed phosphate tailings particles.

[0010] Furthermore, the mass volume ratio of the phosphate tailings and the activator is 5g:3mL~7mL.

[0011] Furthermore, the amount of cellulose used is 4wt.% to 6wt.% of the acid-hydrolyzed phosphate tailings.

[0012] Furthermore, the activation reaction is to stir the mixture at 150 r / min to 250 r / min for 30 min to 60 min.

[0013] Furthermore, the activator is slag acid, and the phosphoric acid content in the slag acid is ≥60wt.%.

[0014] Furthermore, the cellulose is sodium carboxymethyl cellulose.

[0015] Furthermore, the specific method for treating the phosphate tailings is as follows: washing the phosphate tailings with water, drying them at 40°C to 60°C for 3h to 4h, and then crushing and screening them. The particle size of the phosphate tailings after screening is 40 mesh to 80 mesh, thereby obtaining treated phosphate tailings.

[0016] Furthermore, the effective phosphorus content in the phosphate tailings is 0.5wt.% to 1wt.%, the effective magnesium content is 4wt.% to 7wt.%, and the effective calcium content is 8wt.% to 14wt.%.

[0017] The second object of the present invention is to provide acid-hydrolyzed phosphate tailing particles prepared by the above preparation method, wherein the particle size of the acid-hydrolyzed phosphate tailing particles is 2mm-4mm, the strength of the acid-hydrolyzed phosphate tailing particles is ≥15N, and the disintegration rate of the acid-hydrolyzed phosphate tailing particles in water at room temperature for 10 minutes is ≥90%.

[0018] The third object of the present invention is to provide the use of the above-mentioned acid-hydrolyzed phosphate tailing particles in the preparation of trace nutrient fertilizers.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. The present invention uses slag acid as a phosphate tailings activator to react with phosphate tailings to decompose calcium carbonate and magnesium carbonate into the form of calcium oxide and magnesium oxide. At the same time, due to the acidolysis reaction, carbonate ions are converted into carbon dioxide, so that a large number of pore channels are formed on the surface of the phosphate tailings, thereby increasing its specific surface area. Since the ionic bonds are destroyed, water can more easily penetrate into the interior of the phosphate tailings to form liquid bridges. In addition, due to the precipitation of magnesium ions, the mixture of phosphate tailings and slag acid has high viscosity, which promotes granulation while activating nutrients in the phosphate tailings. On this basis, cellulose is innovatively added as an auxiliary agent in the granulation process, which can improve the viscosity of the granulation system and promote granulation on the one hand, and can act as a dispersant in the final granule product on the other hand. Cellulose swells rapidly in water, so that the phosphate tailings particles can be quickly disintegrated, avoiding the problem of difficult disintegration of the granule product due to the excessively high viscosity of the phosphate tailings slag acid mixture.

[0021] 2. The main raw material of the present invention is the by-product of phosphate tailings, with low production cost and simple process. The prepared product has high formation rate, particle strength and solubility, and is rich in phosphorus, calcium and magnesium nutrients. It can be used as a new type of medium-element granular fertilizer and has huge industrial economic value.

[0022] 3. The acid-hydrolyzed phosphate tailings particles of the present invention have good physical properties, the particle size of the acid-hydrolyzed phosphate tailings particles is 2mm-4m, the strength of the acid-hydrolyzed phosphate tailings particles is ≥15N, and the disintegration rate of the acid-hydrolyzed phosphate tailings particles at room temperature in water for 10 minutes is ≥90%, which meets the national standard GB / T20412-2021 calcium magnesium phosphate fertilizer, and the preparation process is simple, the cost is low, and it has broad industrialization potential. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a performance diagram of the acid-hydrolyzed phosphate tailings particles of Examples 1-9 of the present invention and Comparative Examples 1-3. DETAILED DESCRIPTION

[0024] The following will be combined with the data and drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] It should be noted that the professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods. The phosphate tailings and slag acid in the present invention were purchased from Yunnan Phosphate Chemical Group, and sodium carboxymethyl cellulose was purchased from McLean Company.

[0026] In phosphorus chemical production, for downstream applications, the extracted phosphoric acid is concentrated to increase the mass concentration of P2O5 to 42% to 54%. During concentration, as the mass concentration of phosphoric acid increases, the solubility of impurities such as iron, aluminum, magnesium and fluorine contained in the phosphate ore decreases, the supersaturation increases, and crystals are formed with anions such as phosphate to precipitate and form a phosphorus-containing solid suspension, called slag acid. According to statistics, for every ton of wet-process phosphoric acid produced, an average of 0.15 tons of slag acid is produced. Based on this calculation, the amount of slag acid produced nationwide in 2022 will reach 215,000 tons. With the continuous mining of phosphate mines in my country, the grade of phosphate mines continues to decrease, resulting in an increasing amount of slag acid produced as a by-product of wet-process phosphoric acid. There is an urgent need to achieve efficient and value-added utilization of slag acid. Based on this, the present invention provides a method for preparing acid-hydrolyzed phosphate tailings particles, comprising the following steps:

[0027] S1, washing the phosphate tailings with water, drying them at 40°C to 60°C for 3h to 4h, and then crushing and screening them. The particle size of the phosphate tailings after screening is 40 mesh to 80 mesh, and the treated phosphate tailings are obtained;

[0028] S2, mixing the treated phosphate tailings and an activator to form a mixture, stirring at 150r / min-250r / min for 30min-60min to perform an activation reaction, wherein the activation reaction promotes the decomposition of the phosphate tailings, increases the void channels of the phosphate tailings, forms a liquid bridge, and obtains an acid-decomposed phosphate tailings;

[0029] S3. The acid-hydrolyzed phosphate tailings and cellulose are mixed and subjected to a disc granulation process. During the granulation process, water is added to moisten the surface of the composite raw materials and provide dissolution and reaction conditions for the cellulose. The cellulose increases the viscosity of the granulation system, promotes granulation, and increases the disintegration of the phosphate tailings particles, thereby obtaining acid-hydrolyzed phosphate tailings particles.

[0030] The present invention uses slag acid as a phosphorus tailings activator, which is a byproduct of the phosphorus chemical industry, with abundant sources and low cost. It reacts with the phosphorus tailings through strong acid, decomposing calcium carbonate and magnesium carbonate into the form of calcium oxide and magnesium oxide, which are more easily absorbed and utilized by crops in the soil. At the same time, due to the acidolysis reaction, carbonate radicals are converted into carbon dioxide, so that the phosphorus tailings show a large number of pore channels, thereby increasing its specific surface area, and because the ionic bond is destroyed, moisture is more likely to penetrate into the inside of the phosphorus tailings to form a liquid bridge, in addition, due to the precipitation of magnesium ions, the mixture composed of phosphorus tailings and slag acid has a high viscosity, and promotes granulation while activating the nutrients of the phosphorus tailings. On this basis, in the granulation process, cellulose is innovatively added as an auxiliary agent, which can improve the viscosity of the granulation system and promote granulation on the one hand, and can act as a dispersant in the final granule product on the other hand, and cellulose swells rapidly in water, so that the phosphorus tailings particles can be quickly disintegrated, avoiding the problem of the difficulty of disintegration of the granule product due to the high viscosity of the phosphorus tailings slag acid mixture.

[0031] In a specific embodiment, the mass volume ratio of the phosphate tailings and the activator is 5g:3mL~7mL. As a preferred solution of the present invention, the mass volume ratio of the phosphate tailings and the activator can be any ratio between 5g:3mL~7mL, and more preferably, the mass volume ratio of the phosphate tailings and the activator is 5g:6mL; the activator is slag acid, and the phosphoric acid content in the slag acid is ≥60wt.%. The activator used in the present invention is slag acid, a by-product of the phosphorus chemical industry, with a phosphoric acid content of more than 60%. The slag acid is a strong acid, which reacts with the phosphate tailings by acidolysis, decomposes the calcium carbonate and magnesium carbonate in the phosphate tailings, and increases the pore channels and specific surface area.

[0032] In a specific embodiment, the amount of cellulose is 4wt.% to 6wt.% of the acid-hydrolyzed phosphate tailings. As a preferred embodiment of the present invention, the amount of cellulose is any value between 4wt.% and 6wt.% of the acid-hydrolyzed phosphate tailings, and more preferably, the amount of cellulose is 5wt.% of the acid-hydrolyzed phosphate tailings; the cellulose is sodium carboxymethyl cellulose. During the disc granulation process, sodium carboxymethyl cellulose is added in batches, and 1wt.% to 3wt.% of sodium carboxymethyl cellulose is first evenly sprinkled on the raw material mixture to form small particles, and then the remaining raw material mixture and the remaining sodium carboxymethyl cellulose are added simultaneously to continue granulation until a predetermined particle size is reached to obtain phosphate tailing particles.

[0033] In a specific embodiment, the phosphate tailings are byproducts of the production of phosphate fertilizers in the phosphate chemical industry, and the effective phosphorus content in the phosphate tailings is 0.5wt.% to 1wt.%, the effective magnesium content is 4wt.% to 7wt.%, and the effective calcium content is 8wt.% to 14wt.%. The main raw material of the present invention is the byproduct of the phosphate tailings, the production cost is low, the process is simple, the prepared product has a high formation rate, particle strength and solubility, and contains rich phosphorus, calcium, and magnesium nutrients, and can be used as a new type of medium-element granular fertilizer, which has great industrial economic value.

[0034] On the other hand, the present invention provides acid-hydrolyzed phosphate tailing particles prepared by the above preparation method, wherein the particle size of the acid-hydrolyzed phosphate tailing particles is 2mm-4mm, the strength of the acid-hydrolyzed phosphate tailing particles is ≥15N, and the disintegration rate of the acid-hydrolyzed phosphate tailing particles in water at room temperature for 10 minutes is ≥90%.

[0035] In addition, the present invention provides the use of the above-mentioned acid-hydrolyzed phosphate tailing particles in the preparation of trace nutrient fertilizers. The acid-hydrolyzed phosphate tailing particles of the present invention have good physical properties, the particle size of the acid-hydrolyzed phosphate tailing particles is 2mm-4m, the strength of the acid-hydrolyzed phosphate tailing particles is ≥15N, and the disintegration rate of 10min in water at room temperature is ≥90%, which meets the national standard of GB / T20412-2021 calcium magnesium phosphate fertilizer, and the preparation process is simple, the cost is low, and it has broad industrialization potential.

[0036] The invention is further described below through specific examples.

[0037] Example 1

[0038] A method for preparing acid-hydrolyzed phosphate tailing particles comprises the following steps:

[0039] S1, washing the phosphate tailings with water, drying them at 60° C. for 3 h, and then crushing and passing through an 80-mesh sieve to obtain treated phosphate tailings powder;

[0040] S2, respectively weighing 300g of the treated phosphate tailings powder and 180mL of slag acid, then mixing to form a mixture, stirring at 150r / min for 30min to perform an activation reaction, placing the reaction product in an oven at 80°C for 24h, and crushing it to pass through an 80-mesh sieve to obtain an acid-hydrolyzed phosphate tailings powder;

[0041] S3, first put 50wt% of acid-hydrolyzed phosphorus tailings powder into the granulation disk, weigh sodium carboxymethyl cellulose powder according to 5wt% of the mass of the total acid-hydrolyzed phosphorus tailings powder, evenly sprinkle it on the above-mentioned raw materials, and use a brush to continuously clean the raw materials bonded to the wall of the disk to gather them in one place; at the same time, spray water in small amounts multiple times into the granulation disk to moisten the surface of the composite raw materials, providing dissolution and reaction conditions for sodium carboxymethyl cellulose. When the powder absorbs water exceeding the maximum molecular bound water under the action of sodium carboxymethyl cellulose, capillary water will be formed, and the capillary water can be quickly Migrate, and pull the particles around the water droplet to the center of the water droplet, combined with the high viscosity provided by sodium carboxymethyl cellulose, promote the granulation process, and further agglomerate to form micronuclei combined with the effect of centrifugal force; in this process, according to the growth of the micronuclei of the phosphate tailings, add the remaining phosphate tailings and sodium carboxymethyl cellulose to the disc in small amounts and multiple times, and spray water to promote the continuous growth of the micronuclei until there is no dry powder; the granulator continues to rotate for 4 to 5 minutes, so that the particles grow to a suitable size with a smooth and round surface, and are sieved with 2 mm and 4.75 mm square hole sieves to obtain phosphate tailings particles;

[0042] S4. After the prepared phosphate tailings particle product is passed through a 2mm-4mm sieve, it is placed in an oven at 60°C for drying for 4 hours, and then taken out and cooled at room temperature to obtain acid-hydrolyzed phosphate tailings particles.

[0043] Example 2

[0044] A method for preparing acid-hydrolyzed phosphate tailing particles comprises the following steps:

[0045] S1, washing the phosphate tailings with water, drying them at 60° C. for 3 h, and then crushing and passing through an 80-mesh sieve to obtain treated phosphate tailings powder;

[0046] S2, respectively weighing 300g of the treated phosphate tailings powder and 240mL of slag acid, then mixing to form a mixture, stirring at 150r / min for 30min to perform an activation reaction, placing the reaction product in an oven at 80°C for 24h, and crushing it to pass through an 80-mesh sieve to obtain an acid-hydrolyzed phosphate tailings powder;

[0047] S3, first put 50wt% of acid-hydrolyzed phosphorus tailings powder into the granulation disk, weigh sodium carboxymethyl cellulose powder according to 5wt% of the mass of the total acid-hydrolyzed phosphorus tailings powder, evenly sprinkle it on the above-mentioned raw materials, and use a brush to continuously clean the raw materials bonded to the wall of the disk to gather them in one place; at the same time, spray water in small amounts multiple times into the granulation disk to moisten the surface of the composite raw materials, providing dissolution and reaction conditions for sodium carboxymethyl cellulose. When the powder absorbs water exceeding the maximum molecular bound water under the action of sodium carboxymethyl cellulose, capillary water will be formed, and the capillary water can be quickly Migrate, and pull the particles around the water droplet to the center of the water droplet, combined with the high viscosity provided by sodium carboxymethyl cellulose, promote the granulation process, and further agglomerate to form micronuclei combined with the effect of centrifugal force; in this process, according to the growth of the micronuclei of the phosphate tailings, add the remaining phosphate tailings and sodium carboxymethyl cellulose to the disc in small amounts and multiple times, and spray water to promote the continuous growth of the micronuclei until there is no dry powder; the granulator continues to rotate for 4 to 5 minutes, so that the particles grow to a suitable size with a smooth and round surface, and are sieved with 2 mm and 4.75 mm square hole sieves to obtain phosphate tailings particles;

[0048] S4. After the prepared phosphate tailings particle product is passed through a 2mm-4mm sieve, it is placed in an oven at 60°C for drying for 4 hours, and then taken out and cooled at room temperature to obtain acid-hydrolyzed phosphate tailings particles.

[0049] Example 3

[0050] A method for preparing acid-hydrolyzed phosphate tailing particles comprises the following steps:

[0051] S1, washing the phosphate tailings with water, drying them at 60° C. for 3 h, and then crushing and passing through an 80-mesh sieve to obtain treated phosphate tailings powder;

[0052] S2, respectively weighing 300g of the treated phosphate tailings powder and 300mL of slag acid, then mixing to form a mixture, stirring at 150r / min for 30min to perform an activation reaction, placing the reaction product in an oven at 80°C for 24h, and crushing it to pass through an 80-mesh sieve to obtain an acid-hydrolyzed phosphate tailings powder;

[0053] S3, first put 50wt% of acid-hydrolyzed phosphorus tailings powder into the granulation disk, weigh sodium carboxymethyl cellulose powder according to 5wt% of the mass of the total acid-hydrolyzed phosphorus tailings powder, evenly sprinkle it on the above-mentioned raw materials, and use a brush to continuously clean the raw materials bonded to the wall of the disk to gather them in one place; at the same time, spray water in small amounts multiple times into the granulation disk to moisten the surface of the composite raw materials, providing dissolution and reaction conditions for sodium carboxymethyl cellulose. When the powder absorbs water exceeding the maximum molecular bound water under the action of sodium carboxymethyl cellulose, capillary water will be formed, and the capillary water can be quickly Migrate, and pull the particles around the water droplet to the center of the water droplet, combined with the high viscosity provided by sodium carboxymethyl cellulose, promote the granulation process, and further agglomerate to form micronuclei combined with the effect of centrifugal force; in this process, according to the growth of the micronuclei of the phosphate tailings, add the remaining phosphate tailings and sodium carboxymethyl cellulose to the disc in small amounts and multiple times, and spray water to promote the continuous growth of the micronuclei until there is no dry powder; the granulator continues to rotate for 4 to 5 minutes, so that the particles grow to a suitable size with a smooth and round surface, and are sieved with 2 mm and 4.75 mm square hole sieves to obtain phosphate tailings particles;

[0054] S4. After the prepared phosphate tailings particle product is passed through a 2mm-4mm sieve, it is placed in an oven at 60°C for drying for 4 hours, and then taken out and cooled at room temperature to obtain acid-hydrolyzed phosphate tailings particles.

[0055] Example 4

[0056] A method for preparing acid-hydrolyzed phosphate tailing particles comprises the following steps:

[0057] S1, washing the phosphate tailings with water, drying them at 60° C. for 3 h, and then crushing and passing through an 80-mesh sieve to obtain treated phosphate tailings powder;

[0058] S2, respectively weighing 300g of the treated phosphate tailings powder and 360mL of slag acid, then mixing to form a mixture, stirring at 150r / min for 30min to perform an activation reaction, placing the reaction product in an oven at 80°C for 24h, and crushing it to pass through an 80-mesh sieve to obtain an acid-hydrolyzed phosphate tailings powder;

[0059] S3, first put 50wt% of acid-hydrolyzed phosphorus tailings powder into the granulation disk, weigh sodium carboxymethyl cellulose powder according to 5wt% of the mass of the total acid-hydrolyzed phosphorus tailings powder, evenly sprinkle it on the above-mentioned raw materials, and use a brush to continuously clean the raw materials bonded to the wall of the disk to gather them in one place; at the same time, spray water in small amounts multiple times into the granulation disk to moisten the surface of the composite raw materials, providing dissolution and reaction conditions for sodium carboxymethyl cellulose. When the powder absorbs water exceeding the maximum molecular bound water under the action of sodium carboxymethyl cellulose, capillary water will be formed, and the capillary water can be quickly Migrate, and pull the particles around the water droplet to the center of the water droplet, combined with the high viscosity provided by sodium carboxymethyl cellulose, promote the granulation process, and further agglomerate to form micronuclei combined with the effect of centrifugal force; in this process, according to the growth of the micronuclei of the phosphate tailings, add the remaining phosphate tailings and sodium carboxymethyl cellulose to the disc in small amounts and multiple times, and spray water to promote the continuous growth of the micronuclei until there is no dry powder; the granulator continues to rotate for 4 to 5 minutes, so that the particles grow to a suitable size with a smooth and round surface, and are sieved with 2 mm and 4.75 mm square hole sieves to obtain phosphate tailings particles;

[0060] S4. After the prepared phosphate tailings particle product is passed through a 2mm-4mm sieve, it is placed in an oven at 60°C for drying for 4 hours, and then taken out and cooled at room temperature to obtain acid-hydrolyzed phosphate tailings particles.

[0061] Example 5

[0062] A method for preparing acid-hydrolyzed phosphate tailing particles comprises the following steps:

[0063] S1, washing the phosphate tailings with water, drying them at 60° C. for 3 h, and then crushing and passing through an 80-mesh sieve to obtain treated phosphate tailings powder;

[0064] S2, respectively weighing 300g of the treated phosphate tailings powder and 420mL of slag acid, then mixing to form a mixture, stirring at 150r / min for 30min to perform an activation reaction, placing the reaction product in an oven at 80°C for 24h, and crushing it to pass through an 80-mesh sieve to obtain an acid-hydrolyzed phosphate tailings powder;

[0065] S3, first put 50wt% of acid-hydrolyzed phosphorus tailings powder into the granulation disk, weigh sodium carboxymethyl cellulose powder according to 5wt% of the mass of the total acid-hydrolyzed phosphorus tailings powder, evenly sprinkle it on the above-mentioned raw materials, and use a brush to continuously clean the raw materials bonded to the wall of the disk to gather them in one place; at the same time, spray water in small amounts multiple times into the granulation disk to moisten the surface of the composite raw materials, providing dissolution and reaction conditions for sodium carboxymethyl cellulose. When the powder absorbs water exceeding the maximum molecular bound water under the action of sodium carboxymethyl cellulose, capillary water will be formed, and the capillary water can be quickly Migrate, and pull the particles around the water droplet to the center of the water droplet, combined with the high viscosity provided by sodium carboxymethyl cellulose, promote the granulation process, and further agglomerate to form micronuclei combined with the effect of centrifugal force; in this process, according to the growth of the micronuclei of the phosphate tailings, add the remaining phosphate tailings and sodium carboxymethyl cellulose to the disc in small amounts and multiple times, and spray water to promote the continuous growth of the micronuclei until there is no dry powder; the granulator continues to rotate for 4 to 5 minutes, so that the particles grow to a suitable size with a smooth and round surface, and are sieved with 2 mm and 4.75 mm square hole sieves to obtain phosphate tailings particles;

[0066] S4. After the prepared phosphate tailings particle product is passed through a 2mm-4mm sieve, it is placed in an oven at 60°C for drying for 4 hours, and then taken out and cooled at room temperature to obtain acid-hydrolyzed phosphate tailings particles.

[0067] Example 6

[0068] A method for preparing acid-hydrolyzed phosphate tailing particles comprises the following steps:

[0069] S1, washing the phosphate tailings with water, drying them at 60° C. for 3 h, and then crushing and passing through an 80-mesh sieve to obtain treated phosphate tailings powder;

[0070] S2, respectively weighing 300g of the treated phosphate tailings powder and 360mL of slag acid, then mixing to form a mixture, stirring at 150r / min for 30min to perform an activation reaction, placing the reaction product in an oven at 80°C for 24h, and crushing it to pass through an 80-mesh sieve to obtain an acid-hydrolyzed phosphate tailings powder;

[0071] S3, first put 50wt% of acid-hydrolyzed phosphorus tailings powder into the granulation disk, weigh sodium carboxymethyl cellulose powder according to 5wt% of the mass of the total acid-hydrolyzed phosphorus tailings powder, evenly sprinkle it on the above-mentioned raw materials, and use a brush to continuously clean the raw materials bonded to the wall of the disk to gather them in one place; at the same time, spray water in small amounts multiple times into the granulation disk to moisten the surface of the composite raw materials, providing dissolution and reaction conditions for sodium carboxymethyl cellulose. When the powder absorbs water exceeding the maximum molecular bound water under the action of sodium carboxymethyl cellulose, capillary water will be formed, and the capillary water can be quickly Migrate, and pull the particles around the water droplet to the center of the water droplet, combined with the high viscosity provided by sodium carboxymethyl cellulose, promote the granulation process, and further agglomerate to form micronuclei combined with the effect of centrifugal force; in this process, according to the growth of the micronuclei of the phosphate tailings, add the remaining phosphate tailings and sodium carboxymethyl cellulose to the disc in small amounts and multiple times, and spray water to promote the continuous growth of the micronuclei until there is no dry powder; the granulator continues to rotate for 4 to 5 minutes, so that the particles grow to a suitable size with a smooth and round surface, and are sieved with 2 mm and 4.75 mm square hole sieves to obtain phosphate tailings particles;

[0072] S4. After the prepared phosphate tailings particle product is passed through a 2mm-4mm sieve, it is placed in an oven at 60°C for drying for 4 hours, and then taken out and cooled at room temperature to obtain acid-hydrolyzed phosphate tailings particles.

[0073] Example 7

[0074] A method for preparing acid-hydrolyzed phosphate tailing particles comprises the following steps:

[0075] S1, washing the phosphate tailings with water, drying them at 60° C. for 3 h, and then crushing and passing through an 80-mesh sieve to obtain treated phosphate tailings powder;

[0076] S2, respectively weighing 300g of the treated phosphate tailings powder and 360mL of slag acid, then mixing to form a mixture, stirring at 150r / min for 30min to perform an activation reaction, placing the reaction product in an oven at 80°C for 24h, and crushing it to pass through an 80-mesh sieve to obtain an acid-hydrolyzed phosphate tailings powder;

[0077] S3, first put 50wt% of acid-hydrolyzed phosphorus tailings powder into the granulation disk, weigh sodium carboxymethyl cellulose powder according to 6wt% of the mass of the acid-hydrolyzed total phosphorus tailings powder, evenly sprinkle it on the above raw materials, and use a brush to continuously clean the raw materials bonded to the wall of the disk to gather them in one place; at the same time, spray water in small amounts multiple times into the granulation disk to moisten the surface of the composite raw materials, providing dissolution and reaction conditions for sodium carboxymethyl cellulose. When the powder absorbs water exceeding the maximum molecular bound water under the action of sodium carboxymethyl cellulose, capillary water will be formed, and the capillary water can migrate faster. The particles around the water droplet are moved and pulled toward the center of the water droplet. The high viscosity provided by sodium carboxymethyl cellulose promotes the granulation process, and the micronuclei are further agglomerated to form micronuclei by the action of centrifugal force. In this process, according to the growth of the micronuclei of the phosphate tailings, the remaining phosphate tailings and sodium carboxymethyl cellulose are added to the disc in small amounts and multiple times, and water is sprayed to promote the continuous growth of the micronuclei until there is no dry powder. The granulator continues to rotate for another 4 to 5 minutes, so that the particles grow to a suitable size with a smooth and round surface, and are sieved with a 2 mm and 4.75 mm square hole sieve to obtain phosphate tailings particles.

[0078] S4. After the prepared phosphate tailings particle product is passed through a 2mm-4mm sieve, it is placed in an oven at 60°C for drying for 4 hours, and then taken out and cooled at room temperature to obtain acid-hydrolyzed phosphate tailings particles.

[0079] Example 8

[0080] A method for preparing acid-hydrolyzed phosphate tailing particles comprises the following steps:

[0081] S1, washing the phosphate tailings with water, drying them at 60° C. for 3 h, and then crushing and passing through an 80-mesh sieve to obtain treated phosphate tailings powder;

[0082] S2, respectively weighing 300g of the treated phosphate tailings powder and 360mL of slag acid, then mixing to form a mixture, stirring at 150r / min for 30min to perform an activation reaction, placing the reaction product in an oven at 80°C for 24h, and crushing it to pass through an 80-mesh sieve to obtain an acid-hydrolyzed phosphate tailings powder;

[0083] S3, first put 50wt% of acid-hydrolyzed phosphorus tailings powder into the granulation disk, weigh sodium carboxymethyl cellulose powder according to 3wt% of the mass of the total acid-hydrolyzed phosphorus tailings powder, evenly sprinkle it on the above raw materials, and use a brush to continuously clean the raw materials bonded to the wall of the disk to gather them in one place; at the same time, spray water in small amounts multiple times into the granulation disk to moisten the surface of the composite raw materials, providing dissolution and reaction conditions for sodium carboxymethyl cellulose. When the powder absorbs water exceeding the maximum molecular bound water under the action of sodium carboxymethyl cellulose, capillary water will be formed, and the capillary water can migrate faster. The particles around the water droplet are moved and pulled toward the center of the water droplet. The high viscosity provided by sodium carboxymethyl cellulose promotes the granulation process, and the micronuclei are further agglomerated to form micronuclei by the action of centrifugal force. In this process, according to the growth of the micronuclei of the phosphate tailings, the remaining phosphate tailings and sodium carboxymethyl cellulose are added to the disc in small amounts and multiple times, and water is sprayed to promote the continuous growth of the micronuclei until there is no dry powder. The granulator continues to rotate for another 4 to 5 minutes, so that the particles grow to a suitable size with a smooth and round surface, and are sieved with a 2 mm and 4.75 mm square hole sieve to obtain phosphate tailings particles.

[0084] S4. After the prepared phosphate tailings particle product is passed through a 2mm-4mm sieve, it is placed in an oven at 60°C for drying for 4 hours, and then taken out and cooled at room temperature to obtain acid-hydrolyzed phosphate tailings particles.

[0085] Example 9

[0086] A method for preparing acid-hydrolyzed phosphate tailing particles comprises the following steps:

[0087] S1, washing the phosphate tailings with water, drying them at 60° C. for 3 h, and then crushing and passing through an 80-mesh sieve to obtain treated phosphate tailings powder;

[0088] S2, respectively weighing 300g of the treated phosphate tailings powder and 360mL of slag acid, then mixing to form a mixture, stirring at 150r / min for 30min to perform an activation reaction, placing the reaction product in an oven at 80°C for 24h, and crushing it to pass through an 80-mesh sieve to obtain an acid-hydrolyzed phosphate tailings powder;

[0089] S3, first put 50wt% of acid-hydrolyzed phosphorus tailings powder into the granulation disk, weigh sodium carboxymethyl cellulose powder according to 7wt% of the mass of the total acid-hydrolyzed phosphorus tailings powder, evenly sprinkle it on the above raw materials, and use a brush to continuously clean the raw materials bonded to the wall of the disk to gather them in one place; at the same time, spray water in small amounts multiple times into the granulation disk to moisten the surface of the composite raw materials, providing dissolution and reaction conditions for sodium carboxymethyl cellulose. When the powder absorbs water exceeding the maximum molecular bound water under the action of sodium carboxymethyl cellulose, capillary water will be formed, and the capillary water can migrate faster. The particles around the water droplet are moved and pulled toward the center of the water droplet. The high viscosity provided by sodium carboxymethyl cellulose promotes the granulation process, and the micronuclei are further agglomerated to form micronuclei by the action of centrifugal force. In this process, according to the growth of the micronuclei of the phosphate tailings, the remaining phosphate tailings and sodium carboxymethyl cellulose are added to the disc in small amounts and multiple times, and water is sprayed to promote the continuous growth of the micronuclei until there is no dry powder. The granulator continues to rotate for another 4 to 5 minutes, so that the particles grow to a suitable size with a smooth and round surface, and are sieved with a 2 mm and 4.75 mm square hole sieve to obtain phosphate tailings particles.

[0090] S4. After the prepared phosphate tailings particle product is passed through a 2mm-4mm sieve, it is placed in an oven at 60°C for drying for 4 hours, and then taken out and cooled at room temperature to obtain acid-hydrolyzed phosphate tailings particles.

[0091] Comparative Example 1

[0092] A method for preparing phosphate tailings particles comprises the following steps:

[0093] S1, washing the phosphate tailings with water, drying them at 60° C. for 3 h, and then crushing and passing through an 80-mesh sieve to obtain treated phosphate tailings powder;

[0094] S2, first put 50wt% of the phosphate tailings powder into the granulation disk, turn on the disk granulation, and when the granulation disk is rotating, spray water evenly on the above raw materials to make the surface of the composite raw materials wet to form small particles, then add the remaining acid-lyzed phosphate tailings powder simultaneously, and spray water into the granulation disk in small amounts for multiple times, continue granulation, and the granulator continues to rotate for 4 to 5 minutes, so that the particles grow to a suitable size and have a smooth and round surface, and sieve with a 2mm and 4.75mm square hole sieve to obtain phosphate tailings particles;

[0095] S4. After the prepared phosphate tailings particle product is passed through a 2mm-4mm sieve, it is placed in an oven at 60°C for drying for 4 hours, and then taken out and cooled at room temperature to obtain phosphate tailings particles.

[0096] Comparative Example 2

[0097] A method for preparing acid-hydrolyzed phosphate tailing particles comprises the following steps:

[0098] S1, washing the phosphate tailings with water, drying them at 60° C. for 3 h, and then crushing and passing through an 80-mesh sieve to obtain treated phosphate tailings powder;

[0099] S2, respectively weighing 300g of the treated phosphate tailings powder and 180mL of slag acid, then mixing to form a mixture, stirring at 150r / min for 30min to perform an activation reaction, placing the reaction product in an oven at 80°C for 24h, and crushing it to pass through an 80-mesh sieve to obtain an acid-hydrolyzed phosphate tailings powder;

[0100] S3, first put 50wt% of the acid-lyzed phosphate tailing powder into the granulation disk, turn on the disk granulation, and when the granulation disk is rotating, spray water evenly on the above raw materials to make the surface of the composite raw materials wet to form small particles, then add the remaining acid-lyzed phosphate tailing powder simultaneously, and spray water into the granulation disk in small amounts for multiple times, continue granulation, and the granulator continues to rotate for 4 to 5 minutes, so that the particles grow to a suitable size and have a smooth and round surface, and sieve with a 2mm and 4.75mm square hole sieve to obtain phosphate tailing particles;

[0101] S4. After the prepared phosphate tailings particle product is passed through a 2mm-4mm sieve, it is placed in an oven at 60°C for drying for 4 hours, and then taken out and cooled at room temperature to obtain acid-hydrolyzed phosphate tailings particles.

[0102] Comparative Example 3

[0103] A method for preparing acid-hydrolyzed phosphate tailing particles comprises the following steps:

[0104] S1, washing the phosphate tailings with water, drying them at 60° C. for 3 h, and then crushing and passing through an 80-mesh sieve to obtain treated phosphate tailings powder;

[0105] S2, respectively weighing 300g of the treated phosphate tailings powder and 180mL of slag acid, then mixing to form a mixture, stirring at 150r / min for 30min to perform an activation reaction, placing the reaction product in an oven at 80°C for 24h, and crushing it to pass through an 80-mesh sieve to obtain an acid-hydrolyzed phosphate tailings powder;

[0106] S3, first put 50wt% of the acid-hydrolyzed phosphorus tailings powder into the granulation disk, weigh the sodium lignin sulfonate powder according to 5wt% of the mass of the total phosphorus tailings powder, evenly sprinkle it on the above raw materials, and use a brush to continuously clean the raw materials bonded to the wall of the disk to gather them in one place; at the same time, spray water into the granulation disk in small amounts and multiple times to make the surface of the composite raw materials moist, providing dissolution and reaction conditions for sodium lignin sulfonate; according to the growth of the phosphorus tailings micronucleus, add the remaining phosphorus tailings and sodium lignin sulfonate to the disk in small amounts and multiple times and spray water to promote the continuous growth of the micronucleus until there is no dry powder; the granulator continues to rotate for 4-5min to make the particles grow to a suitable size and have a smooth and round surface, and sieve them with 2mm and 4.75mm square hole sieves to obtain phosphorus tailings particles;

[0107] S4. After the prepared phosphate tailings particle product is passed through a 2mm-4mm sieve, it is placed in an oven at 60°C for drying for 4 hours, and then taken out and cooled at room temperature to obtain acid-hydrolyzed phosphate tailings particles.

[0108] The structures of the acid-hydrolyzed phosphate tailing particles prepared in Examples 1-9 are similar in shape and effect. The following takes the acid-hydrolyzed phosphate tailing particles prepared in Example 4 and Comparative Example 2 as examples to illustrate the microstructure of the acid-hydrolyzed phosphate tailing particles prepared in Example 4 and Comparative Example 2, and the results are as follows:

[0109] Compared with Comparative Example 2, Example 4 has a relatively loose structure, many fine pores, and a smoother surface due to the addition of cellulose, and has good swelling properties and granulation rate. However, Comparative Example 2 has a relatively tight structure, and at the same time, due to its own high viscosity, the surface is uneven, and the effect is poor compared with the product with added cellulose.

[0110] The particle product performance evaluation method was performed on the acid-hydrolyzed phosphate tailing particles prepared in Examples 1-9 and Comparative Examples 1-3.

[0111] Among them, the granulation rate: use a 2mm~4mm square hole sieve for screening, and particles with a particle size between 2mm and 4mm are qualified products.

[0112] Granulation rate = m1 / m2*100%; where m1 is the mass of the phosphate tailings particles with a particle size between 2mm and 4mm; m2 is the total mass of the mixed powder material before granulation.

[0113] Particle strength: Take 30 fertilizer particles of uniform size and measure them using a KQ-3 particle strength meter.

[0114] Dissolution rate: Take a certain amount of phosphate tailings particle product, record the mass as m1, soak it in still water at room temperature for 10 minutes, weigh the mass of the sample that does not pass the 1.00mm test sieve, record the mass as m2,

[0115] Dissolution rate = (M1-M2) / M1*100%; where M1 is the mass of the phosphate tailings particles with a particle size between 2mm and 4mm; M2 is the total mass of the mixed powder material before granulation.

[0116] The results are shown in Table 1 and Figure 1 As shown, Figure 1 The performance diagram of the acid-lyzed phosphate tailing particles prepared in Examples 1-9 and Comparative Examples 1-3 of the present invention is shown. It should be noted that since the un-acid-lyzed phosphate tailing cannot be granulated without the addition of sodium carboxymethyl cellulose, the product is a fine powder, so there is no data for Comparative Example 1.

[0117] Table 1 Performance data of acid-hydrolyzed phosphate tailing particles prepared in Examples 1-9 and Comparative Examples 1-3

[0118] Granulation rate (%) Dissolution rate (%) Particle strength (N) Example 1 90.2 65.9 66.9 Example 2 91.4 74.1 55.3 Example 3 92.9 80.7 43.1 Example 4 89.7 87.1 34.6 Example 5 90.6 87.5 25.4 Example 6 90.5 79.8 37.2 Example 7 88.6 88.3 33.7 Example 8 90.7 76.4 35.7 Example 9 88.6 88.6 36.1 Comparative Example 1 0 0 0 Comparative Example 2 94.1 23.4 87.3 Comparative Example 3 88.3 81.5 31.8

[0119] like Figure 1 As shown in Table 1, with the increase of the amount of slag acid, the granulation rate has no obvious change trend, all above 90%, the particle strength shows a downward trend, but all above 25N, and the dissolution rate shows an upward trend with the increase of the amount of slag acid. Starting from Example 4, the dissolution rate is higher than 85%, which meets the national standard of GB / T20412-2021 calcium magnesium phosphate fertilizer. Combining the actual cost and the results in the above figure, Example 4 has the best effect. At the same time, the particle dissolution rate shows an increasing trend with the increase of cellulose dosage. When the dosage reaches 5%, the dissolution rate increases to 85%, and as the dosage continues to increase, the dissolution rate effect is not significantly improved, so the comprehensive effect and cost are optimal when the cellulose dosage is 5%. After replacing cellulose with sodium lignin sulfonate, the dissolution rate is only 81.5%, which fails to meet the standard requirements, proving the necessity of cellulose addition.

[0120] It should be noted that when the present invention involves a numerical range, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in the embodiments, in order to avoid redundancy, the present invention describes a preferred embodiment. Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they know the basic creative concept. Therefore, the attached claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0121] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing acid-hydrolyzed phosphate tailings particles, characterized in that: The following steps are involved: The treated phosphate tailings and an activator are mixed to form a mixture, and an activation reaction is performed. The activation reaction promotes the decomposition of the phosphate tailings, increases the void channels of the phosphate tailings, forms a liquid bridge, and obtains an acid-decomposed phosphate tailings; The acid-hydrolyzed phosphate tailings and cellulose are mixed for granulation. During the granulation process, the cellulose increases the viscosity of the granulation system, promotes granulation and increases the disintegration of the phosphate tailings particles, thereby obtaining the acid-hydrolyzed phosphate tailings particles.

2. The method for preparing acid-hydrolyzed phosphate tailing particles according to claim 1, characterized in that: The mass volume ratio of the phosphate tailings and the activator is 5g:3mL-7mL.

3. The method for preparing acid-hydrolyzed phosphate tailing particles according to claim 1, characterized in that: The amount of cellulose used is 4wt.% to 6wt.% of the acid-hydrolyzed phosphate tailings.

4. The method for preparing acid-hydrolyzed phosphate tailing particles according to claim 1, characterized in that: The activation reaction is to stir the mixture at 150 r / min to 250 r / min for 30 min to 60 min.

5. The method for preparing acid-hydrolyzed phosphate tailing particles according to claim 1, characterized in that: The activator is slag acid, and the phosphoric acid content in the slag acid is ≥60wt.%.

6. The method for preparing acid-hydrolyzed phosphate tailing particles according to claim 1, characterized in that: The cellulose is sodium carboxymethyl cellulose.

7. The method for preparing acid-hydrolyzed phosphate tailing particles according to claim 1, characterized in that: The specific method for treating the phosphate tailings is: washing the phosphate tailings with water, drying them at 40°C to 60°C for 3h to 4h, and then crushing and screening them. The particle size of the phosphate tailings after screening is 40 mesh to 80 mesh, and the treated phosphate tailings are obtained.

8. The method for preparing acid-hydrolyzed phosphate tailing particles according to claim 1, characterized in that: The effective phosphorus content in the phosphate tailings is 0.5wt.% to 1wt.%, the effective magnesium content is 4wt.% to 7wt.%, and the effective calcium content is 8wt.% to 14wt.%.

9. Acid-hydrolyzed phosphate tailing particles prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The particle size of the acid-hydrolyzed phosphate tailing particles is 2 mm to 4 mm, the strength of the acid-hydrolyzed phosphate tailing particles is ≥15N, and the disintegration rate of the acid-hydrolyzed phosphate tailing particles in water at room temperature for 10 minutes is ≥90%.

10. Use of the acid-hydrolyzed phosphate tailing particles according to claim 9 in the preparation of trace nutrient fertilizers.

Citation Information

Patent Citations

  • Method for manufacturing sulphur magnesium fertilizer with high-magnesium phosphor tail slag

    CN101367674A

  • Method for producing composite fertilizer fillers by using phosphorite tailings

    CN102557834A

  • Ammonium magnesium phosphate particle not stratified when mixed and disintegrating in water and preparation method of ammonium magnesium phosphate particle

    CN110372419A

  • Phosphorite pellet containing phosphorite gravity separation tailings and preparation method thereof

    CN117303325A

  • Granular compound fertilizer and its preparing process

    CN1325836A

Cited By

  • Manganese dioxide nanoparticle-modified phosphate tailing composite material as well as preparation method and application thereof

    CN120115118A

  • Manganese dioxide nanoparticles@modified phosphate tailings composite material and preparation method and application thereof

    CN120115118B

  • Medium-trace granular fertilizer prepared from phosphate tailings and preparation method of medium-trace granular fertilizer