Method for synthesizing adsorption sulfuric acid resin from vinyl methacrylate and acrylonitrile

By synthesizing the adsorption of sulfuric acid resin with vinyl methacrylate and acrylonitrile, the acidic adsorption effect is improved by using amide group functional groups, solving the problem of low sulphuric acid adsorption efficiency in the prior art, and achieving efficient sulfuric acid separation effect.

CN118955788APending Publication Date: 2024-11-15SHANDONG JUYOU NEW MATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411282223.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, the resin has a low efficiency in adsorbing sulfuric acid. One gram of dry resin can only adsorb 50% sulfuric acid solution less than 0.2 grams, making it difficult to meet the needs of sulfuric acid separation and treatment in chemical production.

Method used

The method of synthesizing and adsorbing sulfuric acid resin with vinyl methacrylate and acrylonitrile is used to form a resin with an amide group functional group through suspension polymerization and sulfuric acid hydrolysis, thereby improving the acidic adsorption effect.

Benefits of technology

The acidic adsorption amount of the resin is significantly increased. 1 gram of dry resin can adsorb 50 grams of 50% sulfuric acid solution, and the adsorption amount is increased by nearly 50 times, which has a good separation effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005042007350000041
    Figure BDA0005042007350000041
Patent Text Reader

Abstract

The invention discloses a method for synthesizing adsorption sulfuric acid resin from vinyl methacrylate and acrylonitrile, and relates to the technical field of adsorption sulfuric acid resin preparation, and the method specifically comprises the following steps: 1, water phase preparation: heating 400 mL of deionized water to 50-60 DEG C, adding a dispersant, dissolving for 30 min, and adding 100 g of salt and 0.004 g of methylene blue; 2, preparing an oil phase: uniformly stirring and mixing a monomer, an initiator, a pore-foaming agent and a cross-linking agent; according to the method for synthesizing the sulfuric acid adsorption resin from vinyl methacrylate and acrylonitrile, sulfuric acid is hydrolyzed into the sulfuric acid adsorption resin with a functional group with an amide group and a framework with a large long chain, and the functional group of the amide group and acidity have affinity, so that the acid adsorption effect of the resin is effectively improved; according to the invention, 50g of 50% sulfuric acid solution can be adsorbed by 1g of dry resin, and compared with the prior art, the adsorption capacity is increased by nearly 50 times.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparation of adsorbed sulfuric acid resin, in particular to a method for synthesizing adsorbed sulfuric acid resin from vinyl methacrylate and acrylonitrile. Background Art

[0002] A large amount of sulfuric acid is produced during the chemical production process, which needs to be separated and processed. The separation of sulfuric acid and chemical products is a difficult problem. The conventional method is to wash with a large amount of water or neutralize with alkali, both of which will affect the quality and yield of the product.

[0003] Adsorption sulfuric acid resin is a high molecular polymer, also known as adsorption resin, which is mainly used to remove inorganic acids from wastewater, decolorize sugar solution, separate and purify natural products and biochemical products, etc. This resin has a porous three-dimensional structure and can effectively remove impurities such as sulfuric acid, carbon dioxide and inorganic acids from water through adsorption, thereby improving water quality; it can also be used in the chemical industry, environmental wastewater, acid gas adsorption treatment, acid soil remediation and other fields, and has broad prospects.

[0004] In the prior art, conventional resins adsorb sulfuric acid in a small amount. Taking sulfuric acid as an example, 1 gram of dry resin can adsorb less than 0.2 grams of 50% sulfuric acid solution, and the adsorption effect is poor. To this end, the present invention provides a method for synthesizing sulfuric acid adsorption resin from vinyl methacrylate and acrylonitrile to solve the above problem. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a method for synthesizing sulfuric acid adsorption resin from vinyl methacrylate and acrylonitrile, which solves the problems mentioned in the above background technology.

[0006] To achieve the above object, the present invention is implemented by the following technical scheme: a method for synthesizing sulfuric acid adsorption resin from vinyl methacrylate and acrylonitrile, specifically comprising the following steps:

[0007] Step 1: Preparation of aqueous phase: Heat 400 mL of deionized water to 50-60°C, add dispersant, dissolve for 30 minutes, then add 100 g of salt and 0.004 g of methylene blue;

[0008] Step 2, oil phase preparation: stirring and mixing the monomer, initiator, porogen and crosslinking agent;

[0009] Step 3: Pour the oil phase into the water phase for suspension polymerization, then heat up to solidify, cool down to 25-30°C and wash with water;

[0010] Step 4: extract the porogen with ethanol or methanol, and continue drying after extraction to obtain copolymer spheres;

[0011] Step 5: hydrolyze in 6 times 50% sulfuric acid for 2 hours, control the temperature at 80°C, cool to 25°C, wash with water until neutral, and dry in a drying oven at 80°C to obtain sulfuric acid adsorption resin.

[0012] Preferably, in step 1, the dispersant is selected from any one of gelatin, hydroxyethyl cellulose and polyvinylpyrrolidone K30.

[0013] Preferably, the added amount of each dispersant is: 2.4-3.4 g of gelatin, 0.04 g of hydroxyethyl cellulose, and 4 g of polyvinylpyrrolidone k30.

[0014] Preferably, in step 1, auxiliary agents sodium carbonate and magnesium sulfate are also included, and the added amounts are 6 g of sodium carbonate and 16 g of magnesium sulfate.

[0015] Preferably, in step 2, the monomer is acrylonitrile; the initiator is selected from azobisisobutyronitrile, benzoyl peroxide, azobisisobutyronitrile, and benzoyl peroxide in a ratio of 1:1; the crosslinking agent is vinyl methacrylate, and the porogen is selected from one or more of toluene, xylene, No. 200 solvent oil, and n-hexadecane.

[0016] Preferably, the added amount of the monomer is 112.8 to 116.4 parts; the added amount of the initiator is 1.3 to 1.5 parts; and the added amount of the porogen is 60 to 70 parts.

[0017] Preferably, in step three, the specific operation method of heating and curing is: first heat to 65°C and keep warm for 2 hours, then heat to 75°C and keep warm for 3 hours, then heat to 85°C and keep warm for 4 hours, and finally heat to 90°C and keep warm for 2 hours.

[0018] Preferably, in step five, the drying is performed until the moisture content is less than 1%.

[0019] Beneficial Effects

[0020] The present invention provides a method for synthesizing sulfuric acid adsorption resin from vinyl methacrylate and acrylonitrile. Compared with the prior art, the present invention has the following beneficial effects:

[0021] The method for synthesizing sulfuric acid adsorption resin by using vinyl methacrylate and acrylonitrile adopts sulfuric acid to hydrolyze into a resin with a functional group having an amide group and a long-chain skeleton to adsorb inorganic acid. Since the functional group of the amide group has affinity with acidity, the acid adsorption effect of the resin is effectively improved. In the present invention, 1 gram of dry resin can adsorb 50% of sulfuric acid solution, which is 50 grams. Compared with the prior art, the adsorption amount is increased by nearly 50 times, the adsorption amount is greatly improved, and a good separation effect is achieved. DETAILED DESCRIPTION

[0022] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Example 1

[0024] A method for synthesizing sulfuric acid adsorption resin from vinyl methacrylate and acrylonitrile, specifically comprising the following steps:

[0025] Step 1: Preparation of aqueous phase: Heat 400 mL of deionized water to 50°C, add 3.4 g of gelatin, stir and dissolve for 30 min, then add 100 g of salt and 0.004 g of methylene blue;

[0026] Step 2, oil phase preparation: 116.4g acrylonitrile, 3.6g ethylene methacrylate, 70g toluene, 1g azobisisobutyronitrile, 0.3g benzoyl peroxide are mixed evenly;

[0027] Step 3: Pour the oil phase into the water phase for suspension polymerization, then heat to 65°C for 2h, 75°C for 3h, 85°C for 4h, 90°C for 2h, then cool to 25°C for washing;

[0028] Step 4: extract the porogen with ethanol or methanol, and continue drying after extraction to obtain copolymer spheres;

[0029] Step 5: Hydrolyze in 6 times 50% sulfuric acid for 2 hours, control the temperature at 80°C, cool to 25°C, wash with water until neutral, and dry in a drying oven at 80°C until the moisture is less than 1%, to obtain sulfuric acid adsorption resin, the structure of which is:

[0030]

[0031] Example 2

[0032] A method for synthesizing sulfuric acid adsorption resin from vinyl methacrylate and acrylonitrile, specifically comprising the following steps:

[0033] Step 1: Preparation of aqueous phase: Heat 400 mL of deionized water to 50°C, add 0.04 g of hydroxyethyl cellulose, stir and dissolve for 30 minutes, then add 100 g of salt and 0.004 g of methylene blue;

[0034] Step 2, oil phase preparation: 114g acrylonitrile, 6g methacrylate, 65g xylene, 1.2g azobisisobutyronitrile, 0.2g benzoyl peroxide are mixed evenly;

[0035] Step 3: Pour the oil phase into the water phase for suspension polymerization, then heat to 65°C for 2h, 75°C for 3h, 85°C for 4h, 90°C for 2h, then cool to 30°C for washing;

[0036] Step 4: extract the porogen with ethanol or methanol, and continue drying after extraction to obtain copolymer spheres;

[0037] Step 5: Hydrolyze in 6 times 50% sulfuric acid for 3 hours, control the temperature at 80°C, cool to 25°C, wash with water until neutral, and dry in a drying oven at 80°C until the moisture is less than 1%, to obtain sulfuric acid adsorption resin.

[0038] Example 3

[0039] A method for synthesizing sulfuric acid adsorption resin from vinyl methacrylate and acrylonitrile, specifically comprising the following steps:

[0040] Step 1: Preparation of aqueous phase: Heat 400 mL of deionized water to 55°C, add 4 g of polyvinylpyrrolidone K30, stir and dissolve for 30 min, then add 100 g of salt and 0.004 g of methylene blue;

[0041] Step 2, oil phase preparation: 112.8g acrylonitrile, 7.2g ethylene methacrylate, 60g No. 200 solvent oil, 1g azobisisobutyronitrile, 0.3g benzoyl peroxide are mixed evenly;

[0042] Step 3: Pour the oil phase into the water phase for suspension polymerization, then heat to 65°C for 2h, 75°C for 3h, 85°C for 4h, 90°C for 2h, then cool to 25°C for washing;

[0043] Step 4: extract the porogen with ethanol or methanol, and continue drying after extraction to obtain copolymer spheres;

[0044] Step 5: hydrolyze in 6 times 50% sulfuric acid for 4 hours, control the temperature at 80°C, cool to 25°C, wash with water until neutral, and dry in a drying oven at 80°C until the moisture is less than 1%, thereby obtaining sulfuric acid adsorption resin.

[0045] Example 4

[0046] A method for synthesizing sulfuric acid adsorption resin from vinyl methacrylate and acrylonitrile, specifically comprising the following steps:

[0047] Step 1: Preparation of aqueous phase: Heat 400 mL of deionized water to 60°C, add 2.4 g of gelatin to swell for 30 minutes, then add 6 g of sodium carbonate and 16 g of magnesium sulfate mixture, stir and dissolve for 30 minutes, then add 100 g of salt and 0.004 g of methylene blue;

[0048] Step 2, oil phase preparation: 115g acrylonitrile, 5g ethylene methacrylate, 60g n-hexadecane, 1.2g azobisisobutyronitrile, 0.3g benzoyl peroxide are mixed evenly;

[0049] Step 3: Pour the oil phase into the water phase for suspension polymerization, then heat to 65°C for 2h, 75°C for 3h, 85°C for 4h, 90°C for 2h, then cool to 30°C for washing;

[0050] Step 4: extract the porogen with ethanol or methanol, and continue drying after extraction to obtain copolymer spheres;

[0051] Step 5: Hydrolyze in 6 times 50% sulfuric acid for 5 hours, control the temperature at 80°C, cool to 25°C, wash with water to neutrality, and dry in a drying oven at 80°C until the moisture is less than 1%, thereby obtaining sulfuric acid adsorption resin.

[0052] Example 5

[0053] A method for synthesizing sulfuric acid adsorption resin from vinyl methacrylate and acrylonitrile, specifically comprising the following steps:

[0054] Step 1: Preparation of aqueous phase: Heat 400 mL of deionized water to 60°C, add 3 g of gelatin, stir and dissolve for 30 min, then add 100 g of salt and 0.004 g of methylene blue;

[0055] Step 2, oil phase preparation: 114.5g acrylonitrile, 5.5g ethylene methacrylate, 40g toluene, 20g No. 200 solvent oil, 1.2g azobisisobutyronitrile, 0.3g benzoyl peroxide are mixed evenly;

[0056] Step 3: Pour the oil phase into the water phase for suspension polymerization, then heat to 65°C for 2h, 75°C for 3h, 85°C for 4h, 90°C for 2h, then cool to 30°C for washing;

[0057] Step 4: extract the porogen with ethanol or methanol, and continue drying after extraction to obtain copolymer spheres;

[0058] Step 5: Hydrolyze in 6 times 50% sulfuric acid for 5 hours, control the temperature at 80°C, cool to 25°C, wash with water to neutrality, and dry in a drying oven at 80°C until the moisture is less than 1%, thereby obtaining sulfuric acid adsorption resin.

[0059] Adsorption test: 1g of sample was loaded into an adsorption column with a diameter of 30mm. A solution containing 7 times sulfuric acid with a concentration of 50% entered the adsorption column from the inlet, flowed through the adsorbent bed at a flow rate of 15m / h, and flowed out from the outlet of the adsorption column. The sulfuric acid content in the effluent was detected. After the cumulative flow reached the set value, deionized water was used for desorption. After desorption, the residual acid was washed with sodium bicarbonate, and the adsorption amount was detected and calculated. The results are shown in Table 1.

[0060] Table 1

[0061] Example 1 Example 2 Example 3 Example 4 Example 5 <![CDATA[50% sulfuric acid adsorption capacity g > 50 45 43 46 48

[0062] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.

[0063] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0064] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for synthesizing sulfuric acid adsorption resin from vinyl methacrylate and acrylonitrile, characterized in that: The specific steps include: Step 1: Preparation of aqueous phase: Heat 400 mL of deionized water to 50-60°C, add dispersant, dissolve for 30 minutes, then add 100 g of salt and 0.004 g of methylene blue; Step 2, oil phase preparation: stirring and mixing the monomer, initiator, porogen and crosslinking agent; Step 3: Pour the oil phase into the water phase for suspension polymerization, then heat up to solidify, cool down to 25-30°C and wash with water; Step 4: extract the porogen with ethanol or methanol, and continue drying after extraction to obtain copolymer spheres; Step 5: hydrolyze in 6 times 50% sulfuric acid for 2-5 hours, control the temperature at 80°C, cool to 25°C, wash with water until neutral, and dry in a drying oven at 80°C to obtain sulfuric acid adsorption resin.

2. The method for synthesizing sulfuric acid adsorption resin from vinyl methacrylate and acrylonitrile according to claim 1, characterized in that: In the step 1, the dispersant is selected from any one of gelatin, hydroxyethyl cellulose and polyvinylpyrrolidone K30.

3. The method for synthesizing sulfuric acid adsorption resin from vinyl methacrylate and acrylonitrile according to claim 2, characterized in that: The added amounts of each dispersant are: 2.4-3.4 g of gelatin, 0.04 g of hydroxyethyl cellulose, and 4 g of polyvinylpyrrolidone k30.

4. The method for synthesizing sulfuric acid adsorption resin from vinyl methacrylate and acrylonitrile according to claim 3, characterized in that: In the step 1, auxiliary agents sodium carbonate and magnesium sulfate are also included, and the added amounts are 6g of sodium carbonate and 16g of magnesium sulfate.

5. The method for synthesizing sulfuric acid adsorption resin from vinyl methacrylate and acrylonitrile according to claim 1, characterized in that: In the step 2, the monomer is acrylonitrile; the initiator is selected from azobisisobutyronitrile and benzoyl peroxide, and the ratio of azobisisobutyronitrile to benzoyl peroxide is 1:1; the crosslinking agent is vinyl methacrylate, and the porogen is selected from one or more of toluene, xylene, No. 200 solvent oil, and n-hexadecane.

6. The method for synthesizing sulfuric acid adsorption resin from vinyl methacrylate and acrylonitrile according to claim 5, characterized in that: The added amount of the monomer is 112.8 to 116.4 parts; the added amount of the initiator is 1.3 to 1.5 parts; and the added amount of the porogen is 60 to 70 parts.

7. The method for synthesizing sulfuric acid adsorption resin from vinyl methacrylate and acrylonitrile according to claim 1, characterized in that: In the step 3, the specific operation method of heating and curing is: first heat to 65°C and keep warm for 2 hours, then heat to 75°C and keep warm for 3 hours, then heat to 85°C and keep warm for 4 hours, and finally heat to 90°C and keep warm for 2 hours.

8. The method for synthesizing sulfuric acid adsorption resin from vinyl methacrylate and acrylonitrile according to claim 1, characterized in that: In the step 5, drying is performed until the moisture content is less than 1%.

Citation Information

Patent Citations

  • Synthetic method for weak-acid adsorption resin suitable for heavy oil wastewater

    CN102816341A

  • Preparation method of polyamide adsorption resin

    CN105837742A

  • Contamination-resistant large-capacity macroporous weak-acid resin synthesis method

    CN105884967A

  • Preparation method of macroporous acrylic acid weak-base anion exchange resin

    CN113024718A

  • Method for synthesizing acrylic acid series weak-acid cation exchange resin with low transformation expansion rate

    CN117024654A