Acetenyl-derived composites, compositions comprising same, methods of making coatings by same, and methods of making devices comprising coatings

By using ethynyl-derived composites to form a resist coating in semiconductor device manufacturing, the decomposition and flatness problems at high temperatures are solved, and the effects of high heat resistance and low weight loss are achieved. It is suitable for uneven substrates Flattening.

CN118955829APending Publication Date: 2024-11-15MERCK PATENT GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411055085.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2017-12-20
Filing Date
2018-12-17
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

During the manufacturing process of semiconductor devices, in the existing lithography technology, the resist coating is prone to decomposition and weight loss at high temperatures, and it is difficult to form a flat coating on an uneven substrate, especially at the junction of dense and sparse areas. Difficult to maintain high flatness.

Method used

Using an ethynyl-derived composite as the resist lower layer composition, including units A and units B, and forming a composition with solvent, to form a coating by applying and curing on the substrate, reducing additives, improving heat resistance and flatness .

Benefits of technology

The heat resistance and low weight loss of the coating at high temperatures can be realized, and the gaps of the uneven substrate can be effectively filled, which significantly improves the flatness of the coating and reduces the film thickness shrinkage rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955829A_ABST
    Figure CN118955829A_ABST
Patent Text Reader

Abstract

[Problem to be solved] It is an object of the present invention to provide a compound having good heat resistance. Another object of the invention is to provide a coating which has low film shrinkage, good gap filling properties and good flatness. [Solution] The present invention provides an ethynyl-derived complex and a composition comprising the same. Also, the present invention provides a method of manufacturing a coating and a method of manufacturing a device using the same.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention is a divisional application of invention patent application No. 201880082279.9 filed on December 17, 2018, entitled “Ethylene-derived complexes, compositions comprising the same, methods for manufacturing coatings therefrom, and methods for manufacturing devices comprising the coatings”. Technical Field

[0002] The present invention relates to acetylene-derivatized complexes and compositions containing the same, and also to methods for making coatings and devices using the same. Background Art

[0003] In the manufacturing process of devices such as semiconductor devices, photolithography using photoresist (hereinafter referred to as "resist") is generally used for fine processing. Fine processing includes the following steps: forming a thin photoresist layer on a semiconductor substrate such as a silicon wafer; covering the layer with a mask pattern corresponding to the pattern of the target device; exposing the layer to activating light such as ultraviolet light through the mask pattern; developing the exposed layer to obtain a photoresist pattern; etching the substrate using the obtained photoresist pattern as a protective coating, thereby forming fine concavoconvexities corresponding to the above-mentioned pattern.

[0004] Due to the high integration and three-dimensionalization of semiconductors in recent years, it is necessary to further coat a layer on a substrate processed to have a fine concavo-convex pattern and repeat the processing.

[0005] The resist composition and other layer compositions can be applied to the substrate in a liquid form, and can be cured by radiation, heating, etc. to obtain the resist coating and other coatings. The resist coating and other coatings are laminated in such a high-precision environment, and high quality is required in terms of certain properties (e.g., film formation, avoidance of mutual mixing with another layer, etc.).

[0006] Under such circumstances, specific compounds having a carbon-carbon triple bond for resist underlayer compositions have been studied, which can be used together with PGMEA or the like used as a solvent and have excellent solvent resistance, etching resistance, heat resistance and gap filling properties (Patent Document 1).

[0007] Also, specific novolac polymers formed by condensation of bisphenol or bisbenzenefluorene with fluorene have been studied and mentioned for their potential applications as hard masks and dielectric materials in the semiconductor industry (Patent Document 2).

[0008] [Citation List]

[0009] [Patent Document]

[0010] [Patent Document 1] JP2016167047A

[0011] [Patent Document 2] US8952121B2 Summary of the invention

[0012] [Technical issues]

[0013] The inventors believe that the heat-resistant compound can be used in photolithography, for example as a resist underlayer composition. They also believe that the useful compound exhibits less decomposition and / or less weight loss under long-term high temperature conditions, for example, at gradually increasing temperatures. They also believe that the compound can be used in manufacturing processes, and has a smaller film thickness shrinkage when subjected to high temperature baking.

[0014] The substrate after fine and complex processing (for example, stepped substrate) itself may have structures (walls, holes, etc.), which are not uniformly distributed but unevenly distributed (sparse and dense). The inventors believe that the composition is ideal for, for example, semiconductor manufacturing processes, which can be filled in such substrates, and the surface of the coating made of the composition can be flattened. When the substrate has dense and sparse areas, due to surface tension and / or shrinkage during conversion to the coating, it is difficult to flatten the coating formed by the composition on the substrate due to interaction between the components of the composition. As mentioned above, even when the composition of the present invention forms a coating on a substrate with dense and sparse areas, high flatness can be produced. Based on the above concepts, the inventors have found acetylene-derived complexes and compositions comprising them. As another advantage, additives can be reduced in those compositions of the present invention.

[0015] [Solution to the problem]

[0016] The ethynyl-derived complex comprises a unit A and a unit B, wherein

[0017] Unit A is represented by formula (1),

[0018]

[0019] Ar is C 6-41 Aromatic ring,

[0020] R1 is hydrogen, halogen, cyano, unsubstituted C 1-6 Alkyl, substituted with at least one 1-6 The C of the substituent selected from alkyl, halogen and cyano 1-6 Alkyl, unsubstituted C 3-20 aromatic ring, or substituted with at least one C 1-6 The C of the substituent selected from alkyl, halogen and cyano 3-20 Aromatic rings,

[0021] R2 and R3 are each independently hydrogen, halogen, cyano, unsubstituted C 1-6 Alkyl, substituted with at least one 1-6 The C of the substituent selected from alkyl, halogen and cyano 1-6 Alkyl, unsubstituted C 3-20 aromatic ring, or substituted with at least one C 1-6 The C of the substituent selected from alkyl, halogen and cyano 3-20 Aromatic rings,

[0022] R4 is C 1-6 Alkyl, halogen or cyano,

[0023] n1 is an integer, n1 ≥ 1,

[0024] n2 is 0, 1, 2, 3, or 4,

[0025] Unit B is represented by formula (2),

[0026]

[0027] Ring Cy1 is C 5-6 Alicyclic compounds,

[0028] Ph1 and Ph2 are each independently C 6-10 Aromatic hydrocarbon rings, each including two adjacent carbon atoms in the ring Cy1,

[0029] R5 and R6 are each independently hydrogen, halogen, cyano, unsubstituted C 1-6 Alkyl, or C substituted with at least one substituent selected from halogen and cyano 1-6 alkyl,

[0030] The dashed line is a direct bond to another part of the ethynyl-derived complex,

[0031] R7, R8 and R9 are each independently hydrogen, unsubstituted C 1-6 Alkyl, substituted with at least one substituent selected from halogen or cyano 1-6 Alkyl, unsubstituted C 6-16 Aromatic hydrocarbons, substituted with at least one substituent selected from halogen or cyano 6-16 Arene, attached to another unsubstituted C moiety of the ethynyl-derived complex 1-6 Alkylene, connected to another part of the ethynyl derived complex, substituted with at least one substituent selected from halogen or cyano 1-6 alkylene, or a direct bond to another moiety of an ethynyl derived complex, n3 and n4 are independently 0, 1, 2, 3 or 4, and

[0032] n5 is 0 or 1.

[0033] The composition comprises an ethynyl-derivatized complex and a solvent.

[0034] The resist underlayer forming composition consists of this composition.

[0035] A method for making a coating comprises applying a layer of composition on a substrate and curing the layer to form a coating. "On a substrate" includes that the applied layer can be formed on the substrate in direct contact therewith, and an intermediate layer can be interposed between the substrate and the applied layer.

[0036] A method for manufacturing a device, comprising: forming a coating from a composition, forming a layer of a photoresist composition on the coating, curing the photoresist composition to form a photoresist layer, exposing a substrate coated with the photoresist layer, developing the exposed substrate to form a resist pattern, etching using the resist pattern as a mask, and processing the substrate. "On the coating" includes that the formed layer of the photoresist composition can be formed on a layer from the composition in direct contact therewith, and an intermediate layer can be interposed between the formed layer of the photoresist composition and the coating from the composition.

[0037] [Effects of the Invention]

[0038] The composite of the present invention can have good heat resistance. The coating made of the composition of the present invention can also have good heat resistance. For example, when heated after forming the film, the weight loss and film thickness shrinkage can be reduced. And even if the substrate is not flat, those compositions can be filled into the gap of the substrate. The surface of the coating made of the composition can be well flattened. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is an explanatory diagram of a substrate structure used for planarization evaluation.

[0040] Figure 2 It is an explanatory diagram of a substrate structure and a coating thereon used for planarization evaluation. DETAILED DESCRIPTION

[0041] The foregoing summary and the following detailed description are provided to illustrate the present invention and are not intended to limit the invention, as claimed.

[0042] definition

[0043] Unless explicitly limited or stated otherwise, in the following of this specification, the symbols, units, abbreviations and terms defined below have the following meanings.

[0044] When "-", "to" or "~" is used herein to specify a numerical range, the numerical range includes the two numbers indicated before and after the "-" or "~", and the units of the two numbers are the same. For example, "5-25 mol%" means "5 mol% or more and 25 mol% or less".

[0045] As used herein, terms such as "Cx-y," "Cx-Cy," and "Cx" refer to the number of carbon atoms in a molecule or substituent. 1-6 "Alkyl" refers to an alkyl chain having 1 to 6 carbon atoms (eg, methyl, ethyl, propyl, butyl, pentyl, and hexyl).

[0046] When the polymer described herein has multiple repeating units, these repeating units are copolymerized. The copolymerization can be any one selected from alternating copolymerization, random copolymerization, block copolymerization, graft copolymerization, and any combination of these. When the polymer or resin is represented by a chemical structure or chemical formula, n, m, etc. in brackets represent the number of repetitions.

[0047] The temperature unit as indicated herein is Celsius. For example, "20 degrees" means "20 degrees Celsius".

[0048] Acetylene-derived composites

[0049] The present invention provides an ethynyl-derivatized complex comprising a unit A and a unit B. The ethynyl-derivatized complex according to the present invention may comprise one or more units A and one or more units B. For example, the complex may be a polymer.

[0050] Unit A is represented by formula (1).

[0051]

[0052] Ar is independently C 6-41 Ar is preferably phenyl, naphthyl, fluorene, anthracene, 9,9-diphenylfluorene, 9,9-dinaphthylfluorene, phenanthrene, perylene or More preferably, Ar is phenyl, naphthyl, fluorene, phenanthrene, perylene or 9,9-diphenylfluorene. Further more preferably, Ar is phenyl, naphthyl or 9,9-diphenylfluorene.

[0053] R1 is independently hydrogen, halogen, cyano, unsubstituted C 1-6 Alkyl (which may be a linear or branched alkyl, unless otherwise specifically limited or stated, the same hereinafter), substituted with at least one 1-6 The C of the substituent selected from alkyl, halogen and cyano 1-6 Alkyl, unsubstituted C 3-20 aromatic ring, or substituted with at least one C1-6 The C of the substituent selected from alkyl, halogen and cyano 3-20 Aromatic ring. Preferably, R1 is hydrogen, methyl, ethyl, isopropyl, butyl, phenyl, naphthyl, pyrrole, furan, thiophene, imidazole, pyrazole, pyridine, pyrimidine, pyrazine, fluorine or cyano. More preferably, R1 is hydrogen, methyl, ethyl, isopropyl, butyl, phenyl, naphthyl, fluorine or cyano. Further preferably, R1 is hydrogen, methyl, butyl, phenyl, fluorine or cyano. Further more preferably, R1 is hydrogen. C of R1 1-6 Alkyl and C 3-20 The substituents substituted on the aromatic ring are preferably methyl, ethyl, isopropyl, butyl, fluorine or cyano, more preferably methyl, fluorine or cyano. A preferred embodiment of the present invention is that each R1 is unsubstituted.

[0054] R2 and R3 are each independently hydrogen, halogen, cyano, unsubstituted C 1-6 Alkyl, substituted with at least one 1-6 The C of the substituent selected from alkyl, halogen and cyano 1-6 Alkyl, unsubstituted C 3-20 An aromatic ring (preferably an aromatic hydrocarbon ring or a heterocyclic ring), or substituted with at least one C 1-6 The C of the substituent selected from alkyl, halogen and cyano 3-20 Aromatic ring (preferably aromatic hydrocarbon ring or heterocyclic ring). Preferably, R2 and R3 are hydrogen, methyl, ethyl, isopropyl, butyl, phenyl, naphthyl, pyrrole, furan, thiophene, imidazole, pyrazole, pyridine, pyrimidine, pyrazine, fluorine or cyano. More preferably, R2 and R3 are hydrogen, methyl, ethyl, isopropyl, butyl, phenyl, naphthyl, fluorine or cyano. Further preferably, R2 and R3 are hydrogen, methyl, butyl, phenyl, fluorine or cyano. Further more preferably, R2 and R3 are hydrogen. The C of R2 and R3 1-6 Alkyl and C 3-20 The substituents substituted on the aromatic ring are preferably methyl, ethyl, isopropyl, butyl, fluorine or cyano, more preferably methyl, fluorine or cyano. A preferred embodiment of the present invention is that each of R2 and R3 is unsubstituted.

[0055] R4 is independently C 1-6 Preferably, R4 is methyl, ethyl, isopropyl, butyl, fluorine or cyano. More preferably, R4 is methyl, butyl, fluorine or cyano.

[0056] n1 is an integer and n1 ≥ 1. Preferably n1 is 1, 2, 3 or 4. More preferably n1 is 1 or 2.

[0057] n2 is 0, 1, 2, 3 or 4. Preferably n2 is 0, 1 or 2. More preferably n2 is 0.

[0058] Unit B is represented by formula (2).

[0059]

[0060] Ring Cy1 is C 5-6 Alicyclic compounds (cyclopentane or cyclohexane). In one embodiment, the combination of Ph1-Cy1-Ph2 exhibits aromatic properties. In the case where part of the units of formula (2) are replaced by fused aromatic rings (e.g., pyrene), it is believed that the solubility of the entire component will deteriorate.

[0061] Ph1 and Ph2 are each independently C 6-10 Aromatic hydrocarbon rings, each including two adjacent carbons in the ring Cy1. Preferably, Ph1 and Ph2 are each independently phenyl or naphthyl. More preferably, Ph1 and Ph2 are phenyl. For example, in the case where the ring Cy1 is cyclopentane, and Ph1 and Ph2 are phenyl, the combination of the rings Cy1, Ph1 and Ph2 represents fluorene.

[0062] R5 and R6 are each independently hydrogen, halogen, cyano, unsubstituted C 1-6 Alkyl, substituted with at least one substituent selected from halogen (preferably fluorine) and cyano 1-6 Preferably, R5 and R6 are independently methyl, ethyl, isopropyl, butyl, fluorine or cyano. More preferably, R5 and R6 are independently methyl, butyl, fluorine or cyano. A preferred embodiment of the present invention is that each of R5 and R6 is unsubstituted.

[0063] The dashed line is a direct bond to another part of the ethynyl derived complex. Here, "another part of the ethynyl derived complex" does not include 1 unit B from which the dashed line comes out. However, in the case where the ethynyl derived complex according to the present invention includes multiple units B, the dashed line may be bonded to other units B (rather than the unit B from which the dashed line comes out). The dashed line is not bonded to R1, R2 or R3.

[0064] R7, R8 and R9 are each independently hydrogen, unsubstituted C 1-6 Alkyl, substituted with at least one substituent selected from halogen (preferably fluorine) or cyano 1-6 Alkyl, unsubstituted C 6-16 Aromatic hydrocarbon, substituted with at least one substituent selected from halogen (preferably fluorine) or cyano 6-16 Arene, attached to another unsubstituted C moiety of the ethynyl-derived complex 1-6 Alkylene, connected to another part of the ethynyl derived complex, substituted with at least one substituent selected from halogen (preferably fluorine) or cyano 1-6 Alkylene, or a direct bond to another part of the ethynyl derived complex. The above C 1-6Preferred embodiments of the alkyl group are independently methyl, ethyl, isopropyl, butyl, more preferably methyl or butyl. 6-16 Preferred embodiments of the aromatic hydrocarbons are independently phenyl, naphthyl, anthracenyl, phenanthrenyl or pyrenyl. 1-6 Preferred embodiments of alkylene are methylene, ethylene, isopropylene, butylene, more preferably methylene or butylene. Here, "another part of the ethynyl derived complex" does not include one unit B where R7, R8 and R9 are located. However, in the case where the ethynyl derived complex according to the present invention includes multiple units B, R7, R8 or R9 may be bonded to other units B (rather than the units B where they are located). R7, R8 or R9 are not bonded to R1, R2 or R3.

[0065] Preferred embodiments of R7, R8 and R9 are each independently unsubstituted C 6-16 Aromatic hydrocarbons, substituted with at least one substituent selected from halogen or cyano 6-16 Arene, attached to another unsubstituted C moiety of the ethynyl-derived complex 1-6 Alkylene, connected to another part of the ethynyl derived complex, substituted with at least one substituent selected from halogen or cyano 1-6 A more preferred embodiment of R7, R8 and R9 is a phenyl group, a naphthyl group, a methylene group, or a direct bond to another part of the complex derived from the ethynyl group, further preferably a phenyl group or a direct bond to another part of the complex derived from the ethynyl group. A preferred embodiment of the present invention is that each of R7, R8 and R9 is unsubstituted.

[0066] n3 and n4 are each independently 0, 1, 2, 3 or 4. Preferably n3 and n4 are each independently 0, 1 or 2. More preferably n3 and n4 are each independently 0 or 1. Further preferably n3 and n4 are 0.

[0067] n5 is 0 or 1. Preferably n5 is 0.

[0068] The unit A represented by the formula (1) is preferably represented by the following formula (1)'.

[0069]

[0070] Ring Cy2 is cyclopentane.

[0071] Ph3 and Ph4 are each independently C 6-10 Aromatic hydrocarbon ring. Preferably, Ph3 and Ph4 are each independently phenyl or naphthyl. More preferably, Ph3 and Ph4 are phenyl.

[0072] Ph5 and Ph6 are each independently C 6-10 An aromatic hydrocarbon ring, each of which includes two adjacent carbons in the ring Cy2. Preferably, Ph5 and Ph6 are each independently phenyl or naphthyl. More preferably, Ph5 and Ph6 are phenyl.

[0073] The definitions and preferred embodiments of R1, R2 and R3 in formula (1)' are each independently the same as described above.

[0074] For example, the compound on the lower left is an ethynyl-derived complex consisting of 1 unit A and 1 unit B. The compound on the lower left can be interpreted as in formula (1), Ar is 9,9-diphenylfluorene, R1, R2 and R3 are hydrogen, n1=2, n2=0. As shown in the lower right, the 1 bond indicated by the arrow is not used to bond other units. And the compound on the lower left can be interpreted as in formula (2), ring Cy1 is a C5 alicyclic compound, Ph1 and Ph2 are phenyl, R7 is phenyl, and n3, n4 and n5 are 0. Since n5 is 0, R8 and R9 do not exist. The dotted line in formula (2) is bonded to Ar (9,9-diphenylfluorene) in unit A.

[0075]

[0076] For example, the following compound is an ethynyl-derived complex composed of 2 units A and 2 units B. The following compound can be interpreted as in formula (1), Ar is a naphthyl group, R1, R2 and R3 are hydrogen, n1 = 1, n2 = 0. And it can be interpreted as in formula (2), ring Cy1 is a C5 alicyclic compound, Ph1 and Ph2 are phenyl groups, one R7 is a phenyl group, the other R7 is a direct bond to another part of the ethynyl-derived complex (Ar in formula (1)), and n3, n4, n5 are 0. It can be interpreted as the dotted line in formula (2) is bonded to another part of the ethynyl-derived complex (Ar in formula (1)).

[0077]

[0078] For example, the following compound is an ethynyl-derived complex composed of 2 units A and 2 units B. The following compound can be interpreted as in formula (1), Ar is a naphthyl group, R1, R2 and R3 are hydrogen, n1=1, n2=0. And it can be interpreted as in formula (2), ring C1 is a C5 alicyclic compound, P1 and P2 are phenyl groups, R7 is a direct bond to another part of the ethynyl-derived complex (each R7 is bonded to another R7 in another unit B), and n3, n4 and n5 are 0. It can be interpreted as the dotted line in formula (2) is bonded to another part of the ethynyl-derived complex (Ar in formula (1)).

[0079]

[0080] A preferred embodiment of the ethynyl-derivatized complex according to the present invention is described below.

[0081]

[0082] In the above structure, n represents a repeating number (the same applies hereinafter). When the ethynyl-derivatized complex is a polymer (including a dimer), alternating copolymerization is a preferred embodiment.

[0083] For the sake of understanding, exemplary embodiments of ethynyl-derived complexes are described below. These are for illustrative purposes only and are not intended to limit the scope of these inventions.

[0084]

[0085]

[0086]

[0087]

[0088] The concentration of unit A is preferably 30 to 70 mol%, more preferably 40 to 60 mol%, and further preferably 45 to 55 mol%, compared to all units in the ethynyl derived complex according to the present invention. Furthermore, the concentration of unit B is preferably 30 to 70 mol%, more preferably 40 to 60 mol%, and further preferably 45 to 55 mol%, compared to all units in the ethynyl derived complex according to the present invention. One embodiment of the ethynyl derived complex according to the present invention may contain units other than unit A or B. In a preferred embodiment, the molar ratio of unit A to unit B in the ethynyl derived complex is 60:40 to 40:60, more preferably 90:110 to 110:90, and further preferably 100:100.

[0089] The acetylene-derivatized complex preferably comprises units A as terminal groups. These embodiments of the invention have a tendency to be more stable than other embodiments.

[0090] In addition, when the acetylene-derived compound is a polymer, from the viewpoint of increasing the heat resistance of a layer formed by a composition including the acetylene-derived compound, it is preferred that no or almost no secondary carbon atoms and tertiary carbon atoms are contained in the main chain of the polymer. In one embodiment of the present invention, the acetylene-derived compound is a polymer, and when the polymer is synthesized, the amount of the aldehyde derivative (formaldehyde, etc.) is preferably 0 to 30 mol%, more preferably 0 to 15 mol%, more preferably 0 to 5 mol%, and even more preferably 0 mol% based on all components used for synthesis. In order to obtain a polymer containing no or almost no secondary and tertiary carbon atoms in the main chain, the use of a ketone derivative is one of the preferred embodiments of the present invention.

[0091] The present invention provides an electronic material comprising (preferably consisting of) the ethynyl-derived complex of the present invention. The term "electronic material" used in the present invention refers to a material used in the manufacture of an electronic device. In a preferred form of the present invention, the electronic material is used in a coating or layer that is not retained in an electronic device as a final product.

[0092] And the present invention provides a semiconductor material, which comprises (preferably consists of) the ethynyl-derived complex of the present invention. The term "semiconductor material" used in the present invention refers to a material used in the process of manufacturing a semiconductor device. That is, the term is intended to include, for example, a material that forms a coating or layer, such as a photoresist coating or bottom layer, which is removed during the manufacture of the circuit. In a preferred form of the present invention, the semiconductor material is used in a coating or layer that does not remain in the semiconductor device as a final product.

[0093] It is desirable that the impurity content of the electronic material and semiconductor material used as the raw material is 2% or less, preferably 1% or less, more preferably 0.1% or less, and further preferably 0.01% or less. Examples of impurities include raw materials and unreacted precursors used in the synthesis process. When the composition contains an electronic material or a semiconductor material, the term "impurity content" is used to refer to the amount of impurities relative to the amount of the electronic material or the semiconductor material, and the preferred range of the impurity content is as shown above.

[0094] Method for synthesizing ethynyl derivatives

[0095] The detailed procedure of the synthesis method of the ethynyl-derived complex according to the present invention is as described in the synthesis examples given below. Known methods can be combined with them to obtain ethynyl-derived complexes. Precursors can be obtained as described in Patent Document 2. In addition, ethynyl-derived complexes can be obtained by replacing hydroxyl groups with ethynyl-derived groups. The following method for synthesizing ethynyl-derived complexes is an embodiment of the present invention.

[0096]

[0097] Composition

[0098] The present invention provides a composition comprising an ethynyl derived complex according to the present invention and a solvent. As long as the ethynyl derived complex comprises the above-mentioned unit A and unit B, the composition according to the present invention may contain multiple types of ethynyl derived complexes. It is not necessary to limit the number and / or type of unit A and / or unit B. Mixtures of ethynyl derived complexes are acceptable for the scope of the present invention. As described below, for the purpose of understanding, the composition may contain two different ethynyl derived complexes, one ethynyl derived complex having 1 unit A and 1 unit B, and the other ethynyl derived complex having 2 units A and 2 units B.

[0099]

[0100] When a combination of the above compounds is used, these compounds may bond to each other or react independently of each other during the coating formation process.

[0101] The amount of the ethynyl-derived complex is preferably 2 to 60 mass %, more preferably 2 to 30 mass %, further preferably 2 to 20 mass %, further preferably 3 to 10 mass %, relative to the total amount of the composition. Increasing the amount of the solid component relative to the total amount of the composition allows for the formation of a thick coating.

[0102] Solid components other than ethynyl-derivatized compounds

[0103] The composition according to the present invention may further comprise a solid component different from the acetylene derived complex, and the solid component is formed into a coating. The other solid components may be low molecular weight compounds or polymers. When forming a coating, the other solid components may be combined with the acetylene derived complex according to the present invention or may react independently of the acetylene derived complex. These states may exist in a composition mixed together.

[0104] In a preferred embodiment of the present invention, the atoms in one or more solid components in the composition satisfy the following formula (3).

[0105] 1.5≤{total number of atoms / (number of C-number of O)}≤3.5 Formula (3)

[0106] The number of C is the number of carbon atoms in the total number of atoms. The number of O is the number of oxygen atoms in the total number of atoms. The total number of atoms in formula (3) includes the number of hydrogen atoms.

[0107] The composition according to the present invention may consist of an acetylene-derived complex and may contain an acetylene-derived complex and other solid components. As mentioned above, it can be said that the solid component contains an acetylene-derived complex. In order to improve etching resistance, it is preferred that the amount of carbon contained in the composition of the present invention is large.

[0108] Formula (3) is preferably Formula (3)' or Formula (3)".

[0109] 1.5≤{total number of atoms / (number of C-number of O)}≤2.4 (3)'

[0110] 1.8≤{total number of atoms / (number of C-number of O)}≤2.4(3)”

[0111] Solvent

[0112] The solvent used in the present invention may include, for example, water and an organic solvent. And the solvent in the composition according to the present invention may include at least one solvent selected from the group consisting of water, a hydrocarbon solvent, an ether solvent, an ester solvent, an alcohol solvent, and a ketone solvent.

[0113] Examples of the organic solvent include: aliphatic hydrocarbon solvents such as n-pentane, isopentane, n-hexane, isohexane, n-heptane, isoheptane, cyclohexane and methylcyclohexane; aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, trimethylbenzene, methylethylbenzene, n-propylbenzene, isopropylbenzene, diethylbenzene and isobutylbenzene; monohydric alcohol solvents such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, tert-butanol, n-pentanol, isopentanol, 2-methylbutanol, 2-ethylhexanol, n-nonanol, 2,6-dimethylheptanol-4, n-decanol, cyclohexanol, benzyl alcohol , benzyl alcohol, diacetone alcohol and cresol; polyol solvents such as ethylene glycol, propylene glycol, 1,3-butylene glycol, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol and glycerol; ketone solvents such as acetone, methyl ethyl ketone, methyl n-propyl ketone, methyl n-butyl ketone, diethyl ketone, trimethyl nonanone, cyclohexanone, cyclopentanone, methyl cyclohexanone, 2,4-pentanedione, acetonylacetone, acetophenone and fenchone; ether solvents such as ethyl ether, isopropyl ether, n-butyl ether, n-hexyl ether, 2-ethylhexyl ether, dimethyl dioxane, ethylene glycol monomethyl ether, ethylene glycol monomethyl ether, Ethyl ether, ethylene glycol diethyl ether, ethylene glycol mono-n-butyl ether, ethylene glycol mono-n-hexyl ether, ethylene glycol monophenyl ether, ethylene glycol mono-2-ethyl butyl ether, ethylene glycol dibutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol diethyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol di-n-butyl ether, diethylene glycol mono-n-hexyl ether, propylene glycol monomethyl ether (PGME), propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monobutyl ether, tripropylene glycol monomethyl ether, tetrahydrofuran and 2-methyltetrahydrofuran; ester-soluble Solvents such as diethyl carbonate, methyl acetate, ethyl acetate, γ-butyrolactone, γ-valerolactone, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, n-butyl propionate, methyl lactate, ethyl lactate (EL), γ-butyrolactone, n-butyl lactate, n-pentyl lactate, diethyl malonate, dimethyl phthalate, diethyl phthalate, propylene glycol 1-monomethyl ether 2-acetate (PGMEA), propylene glycol monoethyl ether acetate and propylene glycol monopropyl ether acetate; nitrogen-containing solvents such as N-methylformamide; and sulfur-containing solvents such as dimethyl sulfide. Any mixture of these solvents can also be used.

[0114] In particular, cyclohexanone, cyclopentanone, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, propylene glycol 1-monomethyl ether 2-acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, γ-butyrolactone, ethyl lactate and any mixture of these are preferred in terms of storage stability of the solution.

[0115] In terms of solubility of the solute, propylene glycol monomethyl ether, propylene glycol 1-monomethyl ether 2-acetate, ethyl lactate and a mixture of any two solvents selected therefrom are preferred. The mixture of the two solvents is preferably a mixture in a volume ratio of 10:90 to 90:10, more preferably a mixture in a volume ratio of 25:75 to 75:25. For some purposes, propylene glycol 1-monomethyl ether 2-acetate is most preferably used as a solvent.

[0116] Relative to the total amount of the composition, the amount of the organic solvent (or the total amount of two or more organic solvents) is preferably 60 to 98% by mass, more preferably 70 to 98% by mass, and further preferably 80 to 98% by mass. The solvent preferably contains an organic solvent, and the amount of water in the composition is preferably 0.1% by mass or less, and further preferably 0.01% by mass or less. Considering the relationship with another layer or coating, it is preferred that the solvent does not contain water. As one form of the present invention, the amount of water in the composition is preferably 0.00% by mass.

[0117] Surfactants

[0118] The composition according to the present invention may include additives, such as surfactants. Surfactants can be used to reduce pinholes or streaks in the coating made of the composition, and are used to increase the coatability and / or solubility of the composition. Relative to the total amount of the composition, the amount of surfactant (or the total amount of two or more surfactants) is preferably 0 to 5% by mass, and more preferably 0.1 to 3% by mass. Another preferred embodiment of the present invention is that the composition does not include any surfactant (0% by mass).

[0119] Examples of the surfactant include: polyoxyethylene alkyl ether compounds such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether and polyoxyethylene oleyl ether; polyoxyethylene alkyl aryl ether compounds such as polyoxyethylene octylphenol ether and polyoxyethylene nonylphenol ether; polyoxyethylene-polyoxypropylene block copolymer compounds; sorbitan fatty acid ester compounds such as sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan trioleate and sorbitan tristearate; and polyoxyethylene sorbitan fatty acid ester compounds such as polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate and polyoxyethylene sorbitan tristearate. Other examples of the surfactant include: fluorine-containing surfactants such as EFTOP (trade name) EF301, EF303 and EF352 (manufactured by Tohkem Products Corporation), MEGAFACE (trade name) F171, F173, R-08, R-30 and R-2011 (manufactured by DIC Corporation), Fluorad FC430 and FC431 (manufactured by Sumitomo 3M Limited), AsahiGuard (trade name) AG710 (manufactured by Asahi Glass Co., Ltd.) and SURFLON S-382, SC101, SC102, SC103, SC104, SC105 and SC106 (manufactured by Asahi Glass Co., Ltd.); organic siloxane polymers such as KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.).

[0120] Crosslinking agent

[0121] The crosslinking agent may be added to improve the coating forming properties of the coating to be formed, prevent mixing with the upper layer (eg, silicon-containing intermediate layer and resist), and prevent diffusion of low-molecular polymers into the upper layer.

[0122] Exemplary embodiments of crosslinking agents that can be used in the present invention include: melamine, guanamine, glycoluril and urea compounds substituted with at least one group selected from hydroxymethyl, alkoxymethyl and acyloxymethyl; epoxy compounds; thioepoxy compounds; isocyanate compounds; azides; and compounds having double bond-containing groups such as alkenyl ether groups. These can be used as additives or can be introduced into polymer side chains as side groups. Compounds containing hydroxyl groups can also be used as crosslinking agents.

[0123] Examples of the above-mentioned epoxy compounds include tris (2,3-epoxypropyl) isocyanurate, trimethylolmethane triglycidyl ether, trimethylolpropane triglycidyl ether and triethylolethane triglycidyl ether. Exemplary embodiments of melamine compounds include hexamethylol melamine, hexamethoxymethyl melamine, and any mixture of any such compounds. Examples of guanamine compounds include tetramethylol guanamine, tetramethoxymethyl guanamine, and any mixture of any such compounds. Examples of glycoluril compounds include tetramethylol glycoluril, tetramethoxy glycoluril, tetramethoxymethyl glycoluril, and any mixture of any such compounds. Examples of urea compounds include tetramethylol urea and tetramethoxymethyl urea.

[0124] Examples of the compound containing an alkenyl ether group include ethylene glycol divinyl ether and triethylene glycol divinyl ether.

[0125] Examples of the cross-linking agent used in the present invention include those represented by formula (4).

[0126]

[0127] In formula (4), L3 is a direct bond, a substituted or unsubstituted C 1-3 Alkyl, substituted or unsubstituted C 7-16 Aralkyl. L3 is preferably a direct bond, a C1 alkyl or a C 15 The substituent of the alkyl or aralkyl group is preferably hydrogen, methyl, C 6-11 An aryl group or a substituent of formula (5) or formula (6), more preferably a methyl group, a substituent of formula (5) or a substituent of formula (6). In a preferred embodiment, L3 is an unsubstituted C 1-3 Alkyl or unsubstituted C 1-3 Aralkyl.

[0128]

[0129] In formula (4), R 11 It is hydrogen or methyl.

[0130] The following are exemplary embodiments of the cross-linking agent represented by formula (4). The scope of the present invention is not limited thereto.

[0131]

[0132]

[0133] The following is an exemplary embodiment of another crosslinking agent that may be included in the planarization coating forming composition. The scope of the present invention is not limited thereto.

[0134]

[0135] These crosslinking agents are available from, for example, Sanwa Chemical Co., Ltd., Honshu Chemical Industry Co., Ltd., Asahi Yukizai Corporation, and Nippon Carbide Industries Co., Inc.

[0136] In one embodiment of the present invention, the amount of the crosslinking agent is preferably 0 to 300,000 ppm relative to the mass of the entire composition. If the composition contains a crosslinking agent, the amount is preferably 0.1 to 100,000 ppm, more preferably 1 to 50000 ppm, and further preferably 10 to 10,000 ppm.

[0137] Likewise, the composition according to the present invention can also exhibit its effects without adding an effective amount of a crosslinking agent. In this case, the amount of the crosslinking agent is preferably 0 to 20,000 ppm, more preferably 0 to 5,000 ppm, further preferably 0 to 1,000 ppm, and further preferably 0 to 100 ppm relative to the mass of the entire composition.

[0138] In one embodiment of the present invention, the amount of the crosslinking agent is preferably 1 to 200% by mass (more preferably 5 to 100%, further preferably 10 to 40%, further preferably 15 to 25%) relative to the mass of the ethynyl-derived complex (or the total mass of two or more ethynyl-derived complexes) contained in the composition. It is expected that the incorporation of the crosslinking agent into the composition will produce the following effects: the crosslinking agent combines with the ethynyl-derived complex during the coating formation process to control the intramolecular torsion of the entire complex of the crosslinking agent and the compound and increase the flatness of the complex.

[0139] Considering the ease of process control, the present invention can be implemented as an embodiment in which the acetylene-derivatized composite itself forms a coating without adding a crosslinking agent (which means that the amount of the crosslinking agent is 0 mass % relative to the mass of the acetylene-derivatized composite).

[0140] Acid Generator

[0141] One embodiment of the composition according to the present invention may further comprise an acid generator. The amount of the acid generator contained in the composition is preferably 0.1 to 10% by mass, more preferably 1 to 7% by mass, and further preferably 1 to 5% by mass, relative to the mass of the acetylene-derived complex of the present invention (or the total mass of two or more acetylene-derived complexes).

[0142] The acid generator can be a thermal acid generator capable of generating a strong acid when heated. The thermal acid generator (TAG) used in embodiments of the present invention can include one or more thermal acid generators, which, when heated, generate an acid capable of reacting with the complex derived from acetylene and capable of promoting the cross-linking of the complex derived from acetylene. The acid is more preferably a strong acid, such as sulfonic acid. The thermal acid generator is preferably activated at a temperature higher than 80 degrees. Examples of thermal acid generators include: metal-free sulfonium salts, such as triarylsulfonium salts, dialkylarylsulfonium salts and diarylalkylsulfonium salts of strong non-nucleophilic nucleic acids; metal-free iodonium salts, such as alkylaryliodonium salts and diaryliodonium salts of strong non-nucleophilic nucleic acids; ammonium salts, alkylammonium salts, dialkylammonium salts, trialkylammonium salts and tetraalkylammonium salts of strong non-nucleophilic nucleic acids. Covalent thermal acid generators are also considered useful additives, examples of which include 2-nitrobenzyl esters of alkyl or aryl sulfonic acids and other sulfonic acid esters that are thermally decomposed to generate free sulfonic acids. Examples include perfluoroalkyl diaryliodonium and sulfonates. Examples of unstable esters include: nitrobenzyl toluenesulfonates, such as 2-nitrobenzyl toluenesulfonate, 2,4-dinitrobenzyl toluenesulfonate, 2,6-dinitrobenzyl toluenesulfonate, and 4-nitrobenzyl toluenesulfonate; benzenesulfonates, such as 2-trifluoromethyl-6-nitrobenzyl 4-chlorobenzenesulfonate and 2-trifluoromethyl-6-nitrobenzyl 4-nitrobenzenesulfonate; phenolsulfonates, such as phenyl 4-methoxybenzenesulfonate; tri(fluoroalkylsulfonyl)methide quaternary ammonium salts; bis(fluoroalkylsulfonyl)imide quaternary alkylammonium salts; and alkylammonium salts of organic acids, such as the triethylammonium salt of 10-camphorsulfonic acid. Amine salts of various aromatic (anthracene, naphthalene or benzene derivatives) sulfonic acids, including those disclosed in US Pat. No. 3,474,054 B, US Pat. No. 4,200,729 B, US Pat. No. 4,251,665 B and US Pat. No. 5,187,019 B, can be used as TAGs.

[0143] The following are exemplary embodiments of thermal acid generators that may be included in the composition. The scope of the present invention is not limited thereto.

[0144]

[0145] In view of the simplicity of process control, the present invention can be implemented as an embodiment in which no acid generator is added to the composition (which means that the amount of the acid generator is 0 mass % relative to the mass of the acetylene-derivatized complex).

[0146] In one embodiment of the present invention, the amount of the acid generator is preferably 0 to 50,000 ppm, more preferably 0 to 5,000 ppm, further preferably 0 to 1,000 ppm, and further more preferably 0 to 100 ppm, relative to the mass of the entire composition.

[0147] Free Radical Generators

[0148] A free radical generator may be added to the composition to initiate polymerization. The free radical generator generates free radicals when heated, and examples thereof include azo compounds and peroxides. Exemplary embodiments of the free radical generator include organic peroxides, including hydroperoxides, such as diisopropylbenzene hydroperoxide, cumene hydroperoxide, and tert-butyl hydroperoxide; dialkyl peroxides, such as α,α-bis(tert-butylperoxy-m-isopropyl)benzene, dicumyl peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, tert-butylcumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl -2,5-bis(tert-butylperoxy)hexyne-3 and peroxy-2-ethylhexanoic acid tert-butyl ester, peroxide ketones, peroxy ketals such as 4,4-di(tert-butylperoxy)valerate n-butyl ester, diacyl peroxides, peroxydicarbonates and peroxyesters; and azo compounds such as 2,2'-azobisisobutyronitrile, 1,1'-(cyclohexane-1-1-carbonitrile), 2,2'-azobis(2-cyclopropylpropionitrile) and 2,2'-azobis(2,4-dimethylvaleronitrile). These thermal free radical generators can be used alone or in combination, preferably alone. These known free radical generators can be used in the composition, and these free radical generators can be obtained from, for example, NOFCORPORATION.

[0149] In view of the simplicity of process control, the present invention can be implemented as an embodiment in which no free radical generator is added to the composition (which means that the amount of the free radical generator is 0 mass % relative to the mass of the acetylene-derivatized complex).

[0150] As one embodiment, the amount of the free radical generator in the composition of the present invention is preferably 0 to 50,000 ppm, more preferably 0 to 5,000 ppm, further preferably 0 to 1,000 ppm, and further more preferably 0 to 100 ppm, relative to the mass of the entire composition.

[0151] High carbon materials

[0152] The composition according to the present invention may contain a high-carbon material, and the high-carbon material is an organic substance having a large carbon number. By adding a high-carbon material to the composition, the number of atoms of the solid component in the composition can be controlled to satisfy the above formula (3), (3)' and / or (3)".

[0153] One embodiment of the high carbon material is represented by the following formula (7).

[0154]

[0155] Ar1 is a direct bond, C 1-6 Alkyl, C 6-12 Cycloalkyl or C 6-14 Aryl. Ar1 is preferably a direct bond, C 1-6 An alkyl group or a phenyl group, more preferably a direct bond, a linear C3 alkyl group, a linear C6 alkyl group, a tert-butyl group or a phenyl group, and further preferably a direct bond or a phenyl group.

[0156] Ar2 is C 1-6 Alkyl, C 6-12 Cycloalkyl or C 6-14 Ar2 is preferably isopropyl, tert-butyl, C6 cycloalkyl, phenyl, naphthyl, phenanthrenyl or biphenyl, more preferably phenyl.

[0157] R 12 and R 13 Each independently is C 1-6 Alkyl, hydroxy, halogen or cyano. 12 and R 13 Preferably, each is independently methyl, ethyl, propyl, isopropyl, tert-butyl, hydroxy, fluorine, chlorine or cyano, more preferably, each is independently methyl, hydroxy, fluorine or chlorine.

[0158] R 14 is hydrogen, C 1-6 Alkyl or C 6-14 Aryl. 14 Preferably hydrogen, C 1-6 Alkyl or phenyl, more preferably hydrogen, methyl, ethyl, linear C5 alkyl, tert-butyl or phenyl, further preferably hydrogen or phenyl, and further more preferably hydrogen.

[0159] When Ar2 is C 1-6 Alkyl or C 6-14 Aryl and R7 is C 1-6 Alkyl or C 6-14 In case of aromatic groups, Ar2 and R 14 They are optionally linked to each other to form a hydrocarbon ring.

[0160] r and s are each independently 0, 1, 2, 3, 4 or 5. r and s are preferably each independently 0 or 1, and r and s are more preferably each independently 0.

[0161] At least one of the Cy3, Cy4 and Cy5 rings respectively surrounded by dotted lines is an aromatic hydrocarbon ring fused with the adjacent aromatic hydrocarbon ring Ph7, and the total number of carbon atoms of the aromatic hydrocarbon ring and the aromatic hydrocarbon ring Ph7 is preferably C10-14 , more preferably C 10 .

[0162] At least one of the Cy6, Cy7 and Cy= rings respectively surrounded by dotted lines is an aromatic hydrocarbon ring fused with the adjacent aromatic hydrocarbon ring Ph8, and the total number of carbon atoms of the aromatic hydrocarbon ring and the aromatic hydrocarbon ring Ph8 is preferably C 10-14 , more preferably C 10 .

[0163] In formula (7), R 12 , R 13 The bonding position with OH is not limited.

[0164] For example, the compound shown below may have the following structure of formula (7). That is, the aromatic hydrocarbon ring Ph7 and the aromatic hydrocarbon ring Cy5 are fused to each other to form a naphthyl ring, and OH is bonded to the aromatic hydrocarbon ring Cy5. Ar1 is a direct bond, Ar2 and R 14 are each phenyl, and A2 and R 14 Connected to each other to form a hydrocarbon ring (fluorene).

[0165]

[0166] For the purpose of illustration, exemplary compounds of the high carbon material represented by formula (7) are shown below. These examples are not intended to limit the present invention.

[0167]

[0168]

[0169] Other components

[0170] In the composition according to the present invention, other components such as a photopolymerization initiator, an agent for enhancing adhesion to a substrate, a lubricant, a monomer dye, a lower alcohol (C 1-6 The composition comprises a preservative, a surface-leveling agent, a defoamer and a preservative. The amount of these components in the composition is preferably 0.1 to 10% by mass, and more preferably 0.5 to 5% by mass, relative to the amount of the acetylene-derived complex in the composition. In one embodiment of the present invention, the composition does not contain (0% by mass) these components.

[0171] As one embodiment of the present invention, the amount of other components (preferably a photopolymerization initiator) is preferably 0 to 100,000 ppm, more preferably 0 to 5,000 ppm, further preferably 0 to 1,000 ppm, and further preferably 0 to 100 ppm, relative to the mass of the entire composition.

[0172] Composition for forming resist underlayer

[0173] The composition of the present invention is advantageous as a resist underlayer forming composition, for example, for producing patterns by photolithography. Photolithography employs various coatings (also referred to as "layers") with different purposes to form fine patterns. The composition is advantageously used to form such coatings due to its good coating forming properties, gap filling properties, and heat resistance.

[0174] The resist underlayer is a coating formed between a substrate and a photoresist layer. It is not necessary to position the resist underlayer in contact with the photoresist layer. Examples of resist underlayers include planarization coatings, adhesive layers, spin-on carbon coatings (SOC layers), and bottom anti-reflective coatings (BARC layers). A separate resist underlayer may have the functions of these layers or coatings. For example, the resist underlayer may be used as a planarization coating and a BARC layer at the same time. The resist underlayer forming composition is a composition for forming the resist underlayer. A preferred embodiment of the resist underlayer is a planarization coating, and a preferred embodiment of the resist underlayer forming composition is a planarization coating forming composition.

[0175] The composition for forming a planarized coating according to the present invention is such a composition that can be formed as a coating of an upper surface (surface facing the photoresist) located between a substrate and a photoresist coating and having a high flatness. Preferably, an intermediate layer (e.g., an intermediate layer of Si-containing resist, an adhesive layer, a bottom anti-reflective coating or any combination thereof) can be formed on the upper surface (surface facing the photoresist) of the planarized coating, and a photoresist layer can be formed on the intermediate layer. Considering the high etching resistance and easy handling of the composition, the substrate of the present invention can be a flat substrate. Even when the substrate is an uneven substrate, the composition of the present invention fully demonstrates its effect due to having good gap filling performance.

[0176] Since the acetylene-derived composite has high heat resistance, high etching resistance and favorable filling properties, the planarizing coating of the present invention can also be effectively used as a hard mask layer. The hard mask layer is formed to a relatively large thickness (e.g., 1,000 to 3,000 nm); therefore, the fact that the thickness reduction caused by heat is small is conducive to preventing deformation of the coating. In addition, the hard mask layer requires higher etching resistance than ordinary planarizing coatings and spin-on carbon coatings (SOC coatings). A preferred embodiment of the composition for forming the planarizing coating is a composition for forming the hard mask layer.

[0177] Method for producing coating

[0178] One aspect of the method for producing a coating layer according to the present invention will be described.

[0179] As mentioned above, a preferred embodiment is that the resist underlayer according to the present invention is a planarizing coating. The "planarizing coating forming composition" defined in the present invention refers to a composition that can be formed into a coating located between a substrate and a photoresist coating and whose upper surface (the surface facing the photoresist) has a high flatness. Having a high flatness means that the upper surface of the formed planarizing coating is horizontal. When the planarizing coating has a high flatness, the distance between the horizontally positioned bottom surface of the substrate (or the lowest substrate among a plurality of stacked substrates) and the upper surface of the coating varies less. "Flat substrate" refers to a substrate in which the distance between the bottom surface and the top surface is substantially constant (the distance varies in the substrate by 0 to 3%). "Non-flat substrate" broadly refers to a substrate that is not a flat substrate.

[0180] Hereinafter, for easy understanding, the present invention will be described with reference to the accompanying drawings. In order to obtain a composition capable of appropriately forming a coating on a substrate having dense regions and sparse regions, the present inventors used Figure 1 and Figure 2 The substrates shown were examined for the Examples and Comparative Examples. Figure 1 and Figure 2 An imprecise scaling ratio is used in the invention. To facilitate understanding of the invention, reference numeral 1 denotes an island-shaped region extending over 100 μm or more. Reference numeral 2 denotes a sea-shaped region having a width of 100 μm. Reference numeral 3 denotes a dense region extending over 100 μm or more, and wherein a wall structure having a depth of 100 nm is arranged in parallel, with a half pitch of 0.04 μm and a line-to-space ratio of 1:2.5. The substrate is a SiO2 wafer having a sufficient width. Reference numeral 4 denotes the bottom surface of the substrate, and reference numeral 5 denotes the lower portion of the substrate. When the substrate has a plurality of sea-shaped regions or gaps, the height or distance described in the invention is determined according to one of the sea-shaped regions or gaps closest to the bottom surface (except for structures that perforate through the substrate and deviate from the intended design). Reference numeral 6 denotes the top of the substrate. When the substrate has a plurality of tops or gaps, the height or distance described in the invention is determined according to one of the tops farthest from the bottom surface (except for structures that deviate from the intended design). Reference numeral 7 indicates the height between the island-shaped region and the sea-shaped region, and corresponds to the difference between the distance from the top of the island-shaped region to the bottom surface and the distance from the lower portion adjacent to the island-shaped region to the bottom surface. Reference numeral 8 indicates the height between the dense region and the sea-shaped region, and corresponds to the difference between the distance from the top of the dense region to the bottom surface and the distance from the lower portion adjacent to the dense region to the bottom surface. Figure 2As shown in the reference numeral 9 in the figure, a coating is formed. It is difficult for the coating to be completely flat ("completely flat" means that the distance from the coating to the bottom surface is constant). Reference numeral 10 represents the height from the bottom surface of the substrate to the upper surface of the bottom layer formed on the island-shaped area, and reference numeral 11 represents the height from the bottom surface of the substrate to the upper surface of the bottom layer formed on the dense area. The composition according to the present invention is advantageous because it can form a coating on an uneven substrate, so that the difference between the heights represented by reference numerals 10 and 11 becomes smaller (thereby achieving high flatness). When evaluating the composition, the difference between the heights is referred to as the "flattening index."

[0181] Examples of non-planar substrates of the present invention include silicon-containing substrates having a height difference between the top and the bottom (i.e., the difference between the distance from the top to the bottom surface and the distance from the bottom to the bottom surface) of 20 to 10,000 nm. The height difference is preferably 50 to 1,000 nm, more preferably 50 to 500 nm. Preferably, the height difference is determined in a structure in which the top and the bottom are adjacent to each other, as shown in the accompanying drawings numerals 7 and 8. Other examples of non-planar substrates include substrates having walls or contact holes obtained by pretreatment, and also include substrates in which the difference between the distance from the top to the bottom surface and the distance from the bottom to the bottom surface is 30 to 95% (preferably 30 to 80%) of the above-mentioned values. The walls or contact holes can be formed by known techniques such as photolithography, etching or DSA, and preferably have an aspect ratio of 3 to 25 (preferably 5 to 10). A substrate in which only the wall structure is arranged at intervals (see Figure 1 The composition of the present invention is also a non-flat substrate (the region indicated by reference numeral 3 in the figure). For example, when the substrate has both a region where such structures are densely arranged (dense region) and a region where such structures are not present (sparse region), the advantages of the composition of the present invention become apparent. In addition, the composition is suitable for substrates having steps (see Figure 1 The height of the step is preferably 20 to 10,000 nm, more preferably 50 to 1,000 nm, and even more preferably 50 to 500 nm.

[0182] When the coating of the present invention is applied onto a flat substrate (bare wafer) and an underlayer is formed by heating, the thickness of the underlayer may be 20 to 2,000 nm (preferably 100 to 500 nm, more preferably 200 to 400 nm).

[0183] As mentioned above, the substrate used can be a flat substrate or a non-flat substrate. When a non-flat substrate is used, the advantages of the present invention become more obvious.

[0184] The substrate used may be a metal-containing substrate or a silicon-containing substrate. The substrate of the present invention may be a single-layer substrate or a multilayer substrate consisting of a plurality of substrate layers. As the substrate, any known substrate may be used, such as a silicon-coated substrate, a silicon dioxide-coated substrate, a silicon nitride-coated substrate, a silicon wafer substrate (e.g., a SiO2 wafer), a glass substrate, an indium-containing substrate (e.g., an ITO substrate) or a titanium-containing substrate (e.g., a titanium nitride or titanium oxide substrate).

[0185] In the process for manufacturing a semiconductor according to the present invention, the substrate can be configured in any known manner according to the process conditions. Examples of the configuration of the substrate include the multilayer configurations listed below. The left-to-right direction in the table below corresponds to the bottom-to-top direction in the multilayer configuration.

[0186] Silicon wafer substrate

[0187] Silicon wafer substrate / Titanium-containing substrate

[0188] Silicon wafer substrate / titanium-containing substrate / silicon-coated substrate

[0189] Silicon wafer substrate / Titanium-containing substrate / Silicon dioxide-coated substrate

[0190] Silicon wafer substrate / Silicon dioxide coated substrate / Titanium containing substrate

[0191] Silicon nitride substrate

[0192] Silicon nitride substrate / Titanium-containing substrate

[0193] Silicon nitride substrate / titanium-containing substrate / silicon-coated substrate

[0194] Silicon nitride substrate / Titanium-containing substrate / Silicon dioxide-coated substrate

[0195] Silicon nitride substrate / Silicon dioxide coated substrate / Titanium containing substrate

[0196] One substrate to be laminated on another substrate can be formed by a known technique such as CVD. One substrate can be patterned by a known photolithography technique or etching technique. Another substrate can be laminated on a patterned substrate by a known technique such as CVD.

[0197] As an embodiment, the composition of the present invention is applied by a suitable application method such as a spin coater or a coater. When the composition is applied to the substrate, it is preferred that the substrate and the composition according to the present invention are in direct contact with each other, but the composition may be coated with another thin coating (e.g., a substrate modification layer) placed between the composition and the substrate. After applying the composition, ultraviolet irradiation and / or heating are performed to form a lower layer. Preferably, the composition is cured by heating.

[0198] As for the conditions of ultraviolet irradiation of the applied composition, it is preferred to use 100 to 10,000 mJ / cm 2 The composition is irradiated with ultraviolet rays having a wavelength of 10 to 380 nm. The wavelength is preferably 10 to 200 nm, more preferably 100 to 200 nm, even more preferably 125 to 195 nm, and even more preferably 170 to 175 nm. The total radiation dose is preferably 100 to 5,000 mJ / cm 2 , more preferably 200 to 1,000 mJ / cm 2 , even more preferably 300 to 800 mJ / cm 2 The above conditions may be appropriately changed depending on the thickness of the coating to be formed.

[0199] As for the heating conditions adopted when curing the bottom layer by heating, the heating temperature is generally selected from the range of 200 to 600°C (preferably 200 to 500°C, more preferably 220 to 450°C, further preferably 220 to 450, more preferably 250 to 400°C), and the heating time is generally selected from the range of 30 to 180 seconds (preferably 30 to 120 seconds). The heating can be performed in a separate step (stage baking). For example, the heating can be a three-step heating, which includes: a first heating, by which the gap of the substrate is filled and the solvent is removed; a second heating, by which the composition is gently reflowed, thereby forming a coating with high flatness. For example, it is preferred that the first heating is performed at 200 to 300°C for 30 to 120 seconds, the second heating is performed at 300 to 400°C for 30 to 120 seconds, and the third heating is performed at 300 to 500°C for 30 to 120 seconds.

[0200] Ultraviolet irradiation or heating can be carried out in the atmosphere, and its oxygen concentration can be reduced to prevent oxidation of the lower layer forming composition and the lower layer. For example, the oxygen concentration can be adjusted to 1000 ppm or less (preferably 100 ppm or less) by introducing an inactive (inert) gas (N2, Ar, He or a mixture thereof) into the atmosphere.

[0201] Formation of photoresist and other coatings

[0202] A photoresist composition (such as a positive photoresist composition) is applied to the bottom layer formed as described above. The positive photoresist composition described herein refers to a photoresist composition that reacts under light irradiation and whose light irradiated portion has increased solubility in a developer. There is no particular limitation on the photoresist composition used, and any positive photoresist composition, negative photoresist composition, or negative tone development (NTD) photoresist composition can be used as long as the photoresist composition is sensitive to exposure light for pattern formation.

[0203] In the method for manufacturing resist pattern, there may be a coating or layer other than the lower layer and the photoresist coating formed by the lower layer forming composition. An intermediate layer may be inserted between the lower layer and the photoresist coating so that the lower layer and the photoresist coating do not directly contact each other. The intermediate layer is a coating formed between the photoresist coating and the lower layer, and the example of the intermediate layer includes a bottom anti-reflective coating (BARC layer), an inorganic hard mask intermediate layer (such as silicon oxide coating, silicon nitride coating or silicon oxynitride coating) and an adhesive coating. The intermediate layer may be composed of a monolayer or multilayer. A top anti-reflective coating (TARC layer) may be formed on the photoresist coating.

[0204] In the process of manufacturing a device, the layers other than the coating layer may be structured in any known manner according to the conditions of the process. Examples of the structure that can be adopted when the lower layer is a planarization coating layer include the following multilayer structures.

[0205] Substrate / planarization coating / photoresist coating

[0206] Substrate / planarization coating / BARC layer / photoresist coating

[0207] Substrate / planarization coating / BARC layer / photoresist coating / TARC layer

[0208] Substrate / planarization coating / inorganic hard mask intermediate layer / photoresist coating / TARC layer

[0209] Substrate / planarization coating / inorganic hard mask intermediate layer / BARC layer / photoresist coating / TARC layer

[0210] Substrate / planarization coating / adhesive coating / BARC layer / photoresist coating / TARC layer Substrate / substrate modification layer / planarization coating / BARC layer / photoresist coating / TARC layer

[0211] Substrate / substrate modification layer / planarization coating / adhesive coating / BARC layer / photoresist coating / TARC layer

[0212] These layers can be cured by heating and / or exposure after application, or can be formed by known techniques such as CVD. These layers can be removed by known techniques (such as etching), and each layer can be patterned by using the upper layer as a mask.

[0213] In one aspect of the invention, a coating according to the invention may be formed on a non-planar substrate, and another substrate may be formed on the coating. The other substrate may be formed, for example, by a technique such as CVD. The lower substrate and the upper substrate may have the same composition or different compositions. Another layer may also be formed on the upper substrate.

[0214] Patterning and device fabrication

[0215] The photoresist coating is exposed through a given mask. The wavelength of the light used for exposure is not particularly limited. It is preferably exposed with light having a wavelength of 13.5 to 248 nm. In particular, a KrF excimer laser (wavelength: 248 nm), an ArF excimer laser (wavelength: 193 nm) or extreme ultraviolet light (wavelength: 13.5 nm), and more preferably a KrF excimer laser, can be used. These wavelengths may vary within ±1%. If necessary, post-exposure baking can be performed after exposure. The temperature of the post-exposure baking is selected from 80 to 150° C., preferably 100 to 140° C., and the heating time of the post-exposure baking is selected from 0.3 to 5 minutes, preferably 0.5 to 2 minutes.

[0216] Next, development is performed with a developer. When a positive photoresist composition is used, the exposed portion of the positive photoresist layer is removed by development to form a photoresist pattern. For example, a shrink material can be used to make the photoresist pattern finer.

[0217] As a developer for development in the above-mentioned photoresist pattern forming method, a TMAH aqueous solution of 2.38 mass % (acceptable concentration variation is ± 1%) is preferred. Use of such a developer makes it easy to dissolve and remove the planarization coating at room temperature. Additives such as surfactants can be added to the developer. The temperature of the developer is generally selected from 5 to 50° C., preferably 25 to 40° C., and the developing time is generally selected from 10 to 300 seconds, preferably 30 to 60 seconds.

[0218] The intermediate layer, the lower layer and / or the substrate can be patterned by using the obtained photoresist pattern as a mask. For pattern formation, known techniques such as etching (dry etching or wet etching) can be used. For example, the intermediate layer can be etched by using a photoresist pattern as an etching mask, and then the planarization coating and the substrate can be etched by using the obtained intermediate layer pattern as an etching mask to form a pattern on the substrate. Alternatively, the inorganic hard mask intermediate layer can be etched by using a photoresist pattern as an etching mask, the planarization coating can be etched by using the obtained inorganic hard mask intermediate layer pattern as an etching mask, and then the substrate can be etched by using the obtained planarization coating pattern as an etching mask to form a pattern on the substrate. Alternatively, the layer below the photoresist layer (such as the intermediate layer and / or the lower layer) can be etched by using a photoresist pattern as an etching mask, and at the same time, the substrate can be etched by using a photoresist pattern as an etching mask. Wiring can be formed in the substrate using the pattern formed on the substrate.

[0219] For example, the lower layer can be appropriately removed by dry etching with O 2 , CF 4 , CHF 3 , Cl 2 , or BCl 3 . O 2 or CF 4 can be appropriately used.

[0220] Subsequently, if necessary, the substrate is further processed to form an electronic device. This further processing can be accomplished using known methods. After forming the device, if necessary, the substrate is cut into chips, connected to a lead frame and encapsulated with a resin. Preferably, the electronic device is a semiconductor device, a solar cell chip, an organic light emitting device, and an inorganic light emitting device. More preferably, the device is a semiconductor device.

[0221] Example

[0222] Hereinafter, the present invention will be described by examples. These examples are given for illustrative purposes only and are not intended to limit the scope of the present invention. Unless otherwise specified, the term "part" used in the following description refers to mass parts.

[0223] Synthesis Example 1a of P1 Precursor

[0224] Prepare a reaction vessel equipped with an agitator, a condenser (Liebig condenser), a heater, a nitrogen inlet pipe and a temperature controller. 9-fluorenone (200 parts, Tokyo Chemical Industry Co., Ltd., hereinafter referred to as TCI), 9,9-bis (4-hydroxyphenyl) fluorenone (2333 parts, Osaka Gas Chemicals Co., Ltd.) and dichloromethane (10430 parts) are loaded into the reaction vessel, stirred and heated to 40 ° C and maintained at this temperature in a nitrogen atmosphere. Then, trifluoromethanesulfonic acid (92 parts, Mitsubishi Materials Electronic Chemicals Co., Ltd.) and 3-mercaptopropionic acid (6 parts, TCI) dissolved in dichloromethane (200 parts) are slowly added to the reaction vessel, and stirred for 2 hours at 40 ° C to react. After the reaction is completed, the reaction solution is cooled to room temperature. Sufficient water was added to the reaction solution, and excess 9,9-bis(4-hydroxyphenyl)fluorenone was removed by filtration. The precipitate was washed with dichloromethane. Sufficient water was added to the dichloromethane solution to remove trifluoromethanesulfonic acid. The resulting solution was then distilled at 40° C., 10 mmHg to remove dichloromethane, thereby obtaining P1 precursor (2111 parts).

[0225] Mn and Mw were measured by GPC (tetrahydrofuran). Mn was 533 Da. Mw was 674 Da. Molecular weight distribution (Mw / Mn) was 1.26.

[0226] Synthesis Example 1b of P1

[0227] Prepare a reaction vessel equipped with an agitator, a condenser (Liebig condenser), a heater, a nitrogen inlet tube and a temperature controller. P1 precursor (200 parts), potassium carbonate (323 parts) and acetone (616 parts) were loaded into the reaction vessel and kept at 56°C under stirring under a nitrogen atmosphere. Then, 3-bromo-1-propyne (278 parts) was added to the reaction vessel and kept at 56°C for 3 hours under stirring to react. After the reaction was completed, the reaction solution was cooled to normal room temperature. Excess potassium carbonate and its salts were removed by filtration. The precipitate was washed with acetone. Then, the acetone solution was distilled at 40°C, 10mmHg to remove acetone to obtain a dry solid. The obtained dry solid was dissolved in ethyl acetate (820 parts). Sufficient water was added to the ethyl acetate solution to remove metal impurities. The ethyl acetate solution was distilled at 40°C, 10mmHg to remove ethyl acetate to obtain a dry solid. The dry solid (185 parts) was dissolved in acetone (185 parts). Then, methanol (1850 parts) was added to the acetone solution, and filtered to obtain a solid. The solid was dried at 100° C., 10 mmHg. The obtained product was P1 (76 parts).

[0228] Mn and Mw were measured by GPC (tetrahydrofuran). Mn was 789 Da. Mw was 1054 Da.

[0229] The molecular weight distribution (Mw / Mn) was 1.34.

[0230]

[0231] Synthesis Example 2 of P2

[0232] The synthesis was carried out in the same manner as in Synthesis Example 1 except that phenol (TCI) was used instead of 9,9-bis(4-hydroxyphenyl)fluorenone. P2 was obtained.

[0233] Mn and Mw were measured by GPC (tetrahydrofuran). Mn was 703 Da. Mw was 959 Da.

[0234]

[0235] Synthesis Example 3 of P3

[0236] The synthesis was carried out in the same manner as in Synthesis Example 1 except that naphthol (TCI) was used instead of 9,9-bis(4-hydroxyphenyl)fluorenone. P3 was obtained.

[0237] Mn and Mw were measured by GPC (tetrahydrofuran). Mn was 810 Da. Mw was 1,120 Da.

[0238]

[0239] Synthesis Example 4 of P4

[0240] Synthesis was performed in the same manner as in Synthesis Example 1 except that 2,3,6,7-dibenzo-9-fluorenone (Atomax chemicals Co., Ltd.) was used instead of 9-fluorenone and phenol (TCI) was used instead of 9,9-bis(4-hydroxyphenyl)fluorenone. P4 was obtained.

[0241] Mn and Mw were measured by GPC (tetrahydrofuran). Mn was 845 Da. Mw was 1,190 Da.

[0242]

[0243] Synthesis Example 5 of P5

[0244] The synthesis was carried out in the same manner as in Synthesis Example 1 except that anthraquinone (TCI) was used instead of 9-fluorenone and phenol (TCI) was used instead of 9,9-bis(4-hydroxyphenyl)fluorenone. P5 was obtained.

[0245] Mn and Mw were measured by GPC (tetrahydrofuran). Mn was 720 Da. Mw was 1,250 Da.

[0246]

[0247] Preparation Example 1 of Composition 1

[0248] P1 (100 parts) was added to propylene glycol 1-monomethyl ether 2-acetate (PGMEA, 2,500 parts) and stirred. The solution was filtered using a 0.2 μm filter (SLFG025NS, Merck Millipore). The filtered solution was obtained, which was Composition 1.

[0249] Preparation Examples 2 to 7 of Compositions 2 to 7, Comparative Preparation Examples 2 to 4 of Comparative Compositions 2 to 4

[0250] The same procedure as in Preparation Example 1 was carried out except that the components and solvents described in Table 1 below were used instead. Compositions 2 to 7 and comparative compositions 2 to 4 were obtained.

[0251] [Table 1]

[0252] Acetyl-derived complexes (parts) Crosslinking agent (parts) Solvent (parts) Composition 1 P1(100) - PGMEA(1700) Composition 2 P1(100) TM-BIP-ANT(20) PGMEA(2000) Composition 3 P1(100) HM-HAP(20) PGMEA(2000) Composition 4 P2(100) - PGMEA(2000) Composition 5 P3(100) - PGMEA(2000) Composition 6 P4(100) - PGMEA(2000) Composition 7 P5(100) - PGMEA(2000) Comparative composition 1 PA(100) - PGMEA(1700) Comparative composition 2 PB(100) - PGMEA(1700) Comparative composition 3 PC(100) - PGMEA(1700) Comparative composition 4 P1 Precursor (100) - PGMEA(1700)

[0253] TM-BIP-ANT and HM-HAP are as follows.

[0254]

[0255] The compounds PA, PB, PC and PD used in the comparative examples are defined as follows: Described in JP2016167047A, Mw is about 3,500. Described in JP2016167047A, Mw is about 4,500.

[0256] Described in JP2016167047A, Mw is about 4,500.

[0257] Assessment of weight loss

[0258] Each composition was coated on a bare Si wafer (KST World Corp.) using CLEAN TRACK ACT 12 (Tokyo Electron Limited) at 1,500 rpm. The wafer was baked at 250° C. for 60 seconds on a hot plate in an air atmosphere, and then baked at 350° C. for 60 seconds. A coating was thus formed from the composition. The wafer was then further baked at 400° C. for 60 seconds on a hot plate in a nitrogen atmosphere. Then, the coating was scraped off. The obtained solid weight was measured to be A (g). The obtained solid was baked to 400° C. at a rate of 20° C. / min using Thermoplus EVO 2 (Rigaku Corp.) in an air atmosphere. Then, the baked solid weight was measured to be B (g).

[0259] The weight loss (%) was calculated as {100 - (B / A) x 100}. The data are shown in Table 2 below.

[0260] [Table 2]

[0261] Weight loss (%) Gap Filling Composition 1 2.4 A Composition 2 2.8 A Composition 3 2.6 A Composition 4 2.7 A Composition 5 2.4 A Composition 6 2.6 A Composition 7 2.4 A Comparative composition 1 3.1 A Comparative composition 2 4.2 A Comparative composition 3 2.4 B Comparative composition 4 3.5 B

[0262] Gap Fill Evaluation

[0263] Each composition was coated on a stepped SiN wafer (Advanced Materials Technology, Inc.) having a groove of about 10 nm in width and 500 nm in height and having a top of 10 nm in width using a spin coater (MS-150A, Mikasa Co., Ltd.) at 1,500 rpm. The wafer was baked on a hot plate in an air atmosphere at 250° C. for 60 seconds and then at 350° C. for 60 seconds. The wafer was further baked at 400° C. for 60 seconds in a nitrogen atmosphere to produce a coating from the composition.

[0264] A portion of the wafer having the coating layer was prepared, and its groove region was observed by SEM (S-5500, Hitachi High-Tech Fielding Corp.) photograph. The gap filling property of the composition was evaluated as follows. The evaluation results are shown in Table 2.

[0265] A: The composition successfully filled the gaps, so no gaps with voids or holes were found.

[0266] B: The composition fails to sufficiently fill the gaps, so gaps with voids or holes exist.

[0267] Evaluation of film thickness shrinkage

[0268] Each composition was coated on a Si bare wafer (KST World Corp.) using CLEAN TRACK ACT 12 (Tokyo Electron Limited) at 1,500 rpm. The wafer was baked on a hot plate in an air atmosphere at 250° C. for 60 seconds and then at 350° C. for 60 seconds. A coating was thus formed from the composition. The thickness of the coating on the wafer was measured using a Lambda Ace VM-3110 spectroscopic reflectometer (SCREEN Holdings Co., Ltd), and the measured thickness is represented by "Thickness A".

[0269] The wafer was further baked at 400°C for 60 seconds in a nitrogen atmosphere. The thickness of the coating on the wafer was measured using Lambda Ace, and the measured thickness is denoted by "Thickness B".

[0270] The film thickness shrinkage (%) was calculated as {100 - (B / A) x 100}. The data are shown in Table 3 below.

[0271] [Table 3]

[0272] Thickness A(nm) Thickness B(nm) Film thickness shrinkage (%) Flatness index (nm) Composition 1 116 112 3.4 2 Composition 2 118 113 4.2 2 Composition 3 117 113 3.4 4 Composition 4 116 111 4.3 5 Composition 5 118 114 3.4 3 Composition 6 115 111 3.5 4 Composition 7 114 110 3.5 6 Comparative composition 1 118 111 5.9 22 Comparative composition 2 116 108 6.9 21 Comparative composition 3 119 115 3.4 30 Comparative composition 4 117 112 4.3 32

[0273] Evaluation of Flatness Index

[0274] Each composition was coated on a plate using a spin coater (MS-150A, Mikasa Co., Ltd.) at 1,500 rpm. Figure 1 The composition was applied to the SiO2 wafer (non-flat substrate) shown in Figure 1 so that the composition filled the sea-like area and the gaps between the walls of the dense area and covered the island-like area. The wafer was baked at 250°C in air for 60 seconds and then further baked at 350°C for 60 seconds. A coating was thus formed from the composition. Under a nitrogen atmosphere, the wafer was further baked at 400°C for 60 seconds. A portion of the wafer with the coating was prepared and a SEM (S-5500, Hitachi High-Tech Fielding Corp.) photograph was taken.

[0275] The flatness index was measured in the SEM images ( Figure 2 The data are shown in Table 3.

[0276] [reference numerals list]

[0277] 1. Island area of ​​the substrate

[0278] 2. Sea-like area of ​​the substrate

[0279] 3. Dense areas of the substrate

[0280] 4. Substrate bottom surface

[0281] 5. Lower part of substrate

[0282] 6. Top of substrate

[0283] 7. Height between island-like area and sea-like area

[0284] 8. Height between dense area and sea-like area

[0285] 9. The formed flat coating

[0286] 10. The height between the top of the island and the bottom surface of the substrate

[0287] 11. The height between the top of the dense region and the bottom surface of the substrate.

Claims

1. A method for synthesizing an acetylene-derived complex, comprising: The following components were reacted: Among them, Cy1 is C 5-6 Alicyclic compounds, Ph1 and Ph2 are each independently C 6-10 Aromatic hydrocarbon rings, each including two adjacent carbon atoms in the ring Cy1, R5 and R6 are each independently hydrogen, halogen, cyano, unsubstituted C 1-6 Alkyl, or C substituted with at least one substituent selected from halogen and cyano 1-6 alkyl, R8 and R9 are each independently hydrogen, unsubstituted C 1-6 Alkyl, substituted with at least one substituent selected from halogen or cyano 1-6 Alkyl, unsubstituted C 6-16 Aromatic hydrocarbons, substituted with at least one substituent selected from halogen or cyano 6-16 Arene, attached to another unsubstituted C moiety of the ethynyl-derived complex 1-6 Alkylene, attached to another moiety of the ethynyl derived complex, substituted with at least one substituent selected from halogen or cyano 1-6 an alkylene group, or a direct bond to another part of an ethynyl derived complex, n3 and n4 are each independently 0, 1, 2, 3 or 4, n5 is 0 or 1, Ar is each independently C 6-41 Aromatic ring, R4 is each independently C 1-6 Alkyl, halogen or cyano, n1 is 1, 2, 3, or 4, and n2 is 0, 1, 2, 3, or 4; Thus, the precursor is obtained, and replacing hydroxyl groups with ethynyl-derived groups; The synthesized ethynyl-derivatized complex is a polymer.

2. The synthesis method according to claim 1, wherein the acetylene complex is described by the following formula: in, Cy1 is C 5-6 Alicyclic compounds, Ph1 and Ph2 are each independently C 6-10 Aromatic hydrocarbon rings, each including two adjacent carbon atoms in the ring Cy1, R5 and R6 are each independently hydrogen, halogen, cyano, unsubstituted C 1-6 Alkyl, or C substituted with at least one substituent selected from halogen and cyano 1-6 alkyl, R8 and R9 are each independently hydrogen, unsubstituted C 1-6 Alkyl, substituted with at least one substituent selected from halogen or cyano 1-6 Alkyl, unsubstituted C 6-16 Aromatic hydrocarbons, substituted with at least one substituent selected from halogen or cyano 6-16 Arene, attached to another unsubstituted C moiety of the ethynyl-derived complex 1-6 Alkylene, attached to another moiety of the ethynyl derived complex, substituted with at least one substituent selected from halogen or cyano 1-6 an alkylene group, or a direct bond to another part of an ethynyl derived complex, n3 and n4 are each independently 0, 1, 2, 3 or 4, n5 is 0 or 1, Ar is each independently C 6-41 Aromatic ring, R4 is each independently C 1-6 Alkyl, halogen or cyano, n1 is 1, 2, 3, or 4, n2 is 0, 1, 2, 3, or 4, R1 is each independently hydrogen, halogen, cyano, unsubstituted C 1-6 Alkyl, substituted with at least one 1-6 The C of the substituent selected from alkyl, halogen and cyano 1-6 Alkyl, unsubstituted C 3-20 aromatic ring, or substituted with at least one C 1-6 The C of the substituent selected from alkyl, halogen and cyano 3-20 Aromatic rings, R2 and R3 are each independently hydrogen, halogen, cyano, unsubstituted C 1-6 Alkyl, substituted with at least one 1-6 The C of the substituent selected from alkyl, halogen and cyano 1-6 Alkyl, unsubstituted C 3-20 aromatic ring, or substituted with at least one C 1-6 The C of the substituent selected from alkyl, halogen and cyano 3-20 Aromatic rings, and The dashed straight line is a direct bond to another part of the ethynyl-derived complex.

3. The synthesis method according to claim 1, wherein the group derived from the ethynyl group replacing the hydroxyl group is represented by the following formula: in, R1 is each independently hydrogen, halogen, cyano, unsubstituted C 1-6 Alkyl, substituted with at least one 1-6 The C of the substituent selected from alkyl, halogen and cyano 1-6 Alkyl, unsubstituted C 3-20 aromatic ring, or substituted with at least one C 1-6 The C of the substituent selected from alkyl, halogen and cyano 3-20 Aromatic rings, R2 and R3 are each independently hydrogen, halogen, cyano, unsubstituted C 1-6 Alkyl, substituted with at least one 1-6 The C of the substituent selected from alkyl, halogen and cyano 1-6 Alkyl, unsubstituted C 3-20 aromatic ring, or substituted with at least one C 1-6 The C of the substituent selected from alkyl, halogen and cyano 3-20 Aromatic ring.

4. The synthesis method according to claim 2, wherein Ph1 and Ph2 are each independently phenyl or naphthyl, n3 and n4 are 0, or R1, R2 and R3 are hydrogen.

5. The synthesis method according to claim 1, wherein the main chain of the synthesized polymer contains no or almost no secondary carbon and tertiary carbon.

6. The synthesis method according to claim 1, wherein an aldehyde derivative is optionally used when synthesizing the polymer, and the amount of the aldehyde derivative is 0 to 30 mol% based on all components used for the synthesis.

7. The synthesis method according to claim 1, wherein the Mw of the synthesized polymer is 959 to 1,250 Da.

8. A method for producing a composition, wherein the composition comprises the ethynyl-derivatized complex according to claim 1, and a solvent.

9. The method for producing a composition according to claim 8, wherein the solvent comprises at least one solvent selected from the group consisting of water, hydrocarbon solvents, ether solvents, ester solvents, alcohol solvents, and ketone solvents.

10. The method for producing a composition according to claim 8, wherein the solvent comprises at least one solvent selected from the group consisting of water, cyclohexanone, cyclopentanone, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, propylene glycol 1-monomethyl ether 2-acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, γ-butyrolactone, ethyl lactate, or any mixture of these solvents.

11. The method for preparing a composition according to claim 8, wherein the amount of the acetylene-derived complex is 2 to 60% by mass relative to the total amount of the composition; Optionally, the amount of the organic solvent is 60 to 98% by mass relative to the total amount of the composition.

12. The method for preparing a composition according to claim 8, wherein one or more solid components in the composition satisfy the following formula (3): 1.5≤{total number of atoms / (number of C-number of O)}≤3.5 Formula (3), The C number is the number of carbon atoms, and The O number is the number of oxygen atoms.

13. The method for preparing a composition according to claim 8, wherein the composition comprises at least one additive selected from the group consisting of a surfactant, a cross-linking agent, an acid generator, a free radical generator, a high carbon material, a photopolymerization initiator, and an agent for enhancing adhesion to a substrate; Optionally, the composition comprises at least one selected from the group consisting of: a crosslinking agent at a concentration of 0 to 300,000 ppm, a photopolymerization initiator at a concentration of 0 to 100,000 ppm, an acid generator at a concentration of 0 to 50,000 ppm, and a free radical generator at a concentration of 0 to 50,000 ppm; or Optionally, the amount of the surfactant is 0 to 5% by mass relative to the total amount of the composition.

14. The method for producing a composition according to claim 8, wherein the composition is a composition for forming a resist underlayer.

15. A method for making a coating, comprising: applying a layer of the composition made according to claim 8 over the substrate; and curing the layer to form a coating; Optionally, the substrate beneath the produced coating is a flat substrate or a non-flat substrate.

16. The method for manufacturing a coating according to claim 15, wherein the conditions for curing the composition include irradiating with ultraviolet light having a wavelength of 10 to 380 nm, or heating at 200 to 600 degrees Celsius for 30 to 180 seconds.

17. A method for manufacturing a device, comprising: The coating is produced by the method of claim 16, forming a layer of photoresist composition over the coating; curing the photoresist composition to form a photoresist layer; exposing a substrate coated with a photoresist layer; developing the exposed substrate to form a resist pattern; performing etching using the resist pattern as a mask; and The substrate is processed.

18. The method for manufacturing a device according to claim 17, further comprising forming wiring on the processed substrate.

19. A method for synthesizing an acetylene-derived complex, comprising: The following components were reacted: Among them, Cy1 is C 5-6 Alicyclic compounds, Ph1 and Ph2 are each independently C 6-10 Aromatic hydrocarbon rings, each including two adjacent carbon atoms in the ring Cy1, R5 and R6 are each independently hydrogen, halogen, cyano, unsubstituted C 1-6 Alkyl, or C substituted with at least one substituent selected from halogen and cyano 1-6 alkyl, R8 and R9 are each independently hydrogen, unsubstituted C 1-6 Alkyl, substituted with at least one substituent selected from halogen or cyano 1-6 Alkyl, unsubstituted C 6-16 Aromatic hydrocarbons, substituted with at least one substituent selected from halogen or cyano 6-16 Arene, attached to another unsubstituted C moiety of the ethynyl-derived complex 1-6 Alkylene, attached to another moiety of the ethynyl derived complex, substituted with at least one substituent selected from halogen or cyano 1-6 an alkylene group, or a direct bond to another part of an ethynyl derived complex, n3 and n4 are each independently 0, 1, 2, 3 or 4, n5 is 0 or 1, Ar is each independently C 6-41 Aromatic ring, R4 is each independently C 1-6 Alkyl, halogen or cyano, n1 is 1, 2, 3, or 4, and n2 is 0, 1, 2, 3, or 4; Thus, the precursor is obtained, and replacing hydroxyl groups with ethynyl-derived groups; The synthesized ethynyl-derived complex is a polymer of unit A and unit B, wherein the molar ratio of unit A represented by formula (1) to unit B represented by formula (2) in the ethynyl-derived complex is 60:40 to 40:60, The unit A is represented by the following formula (1): wherein Ar, R4, n1 and n2 are each independently as defined above; R1 is each independently hydrogen, halogen, cyano, unsubstituted C 1-6 Alkyl, substituted with at least one 1-6 The C of the substituent selected from alkyl, halogen and cyano 1-6 Alkyl, unsubstituted C 3-20 aromatic ring, or substituted with at least one C 1-6 The C of the substituent selected from alkyl, halogen and cyano 3-20 Aromatic rings, R2 and R3 are each independently hydrogen, halogen, cyano, unsubstituted C 1-6 Alkyl, substituted with at least one 1-6 The C of the substituent selected from alkyl, halogen and cyano 1-6 Alkyl, unsubstituted C 3-20 aromatic ring, or substituted with at least one C 1-6 The C of the substituent selected from alkyl, halogen and cyano 3-20 Aromatic rings, Unit B is represented by the following formula (2): Cy1, Ph1, Ph2, R5, R6, R8, R9, n3, n4 and n5 are each independently as defined above; The dashed straight line is a direct bond to another part of the ethynyl-derived complex; R7 is a direct bond to another portion of the ethynyl-derived complex; Optionally, the concentration of unit A is 30-70 mol% compared to the total units in the ethynyl-derived complex, and the concentration of unit B is 30-70 mol% compared to the total units in the ethynyl-derived complex.

20. The synthesis method according to claim 19, wherein unit A is represented by formula (1)': wherein R1, R2 and R3 are each independently as described in claim 19, cycloCy2 is cyclopentane, Ph3 and Ph4 are each independently C 6-10 an aromatic hydrocarbon ring, and Ph5 and Ph6 are each independently C 6-10 Aromatic ring.