Phenolic resin, epoxy resin and cured product thereof
By introducing benzaldehyde structure into phenolic resin and reacting with epichlorohydrin to prepare epoxy resin, the problem of insufficient stability of epoxy resin packaging materials in high temperature and humidity environments is solved, and higher glass transition temperature and more The low water absorption rate meets the high temperature and humidity resistance of semiconductor materials.
Patent Information
- Application Number
- CN202411034233.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-05
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-07-05
AI Technical Summary
The existing epoxy resin packaging materials are insufficient in high temperature and humidity environments, and it is difficult to meet the high temperature, humidity and heat resistance performance requirements of semiconductor materials in new energy vehicles, consumer electronics and other industries.
By introducing benzaldehyde structures, especially hydroxyl or trifluoromethyl substituted benzaldehyde into the phenolic resin, a phenolic resin with excellent high temperature, humidity and heat resistance is formed, and an epoxy resin is prepared with epichlorohydrin to form a high glass epoxy resin cured substances with transition temperature and low water absorption.
It significantly improves the high temperature, humidity and heat resistance of epoxy resin packaging materials, meets the performance requirements of integrated circuits and semiconductor devices, and provides higher glass transition temperature and lower water absorption.
Smart Images

Figure BDA0004970642940000011 
Figure BDA0004970642940000021 
Figure BDA0004970642940000022
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer curing resin materials, and specifically relates to a phenolic resin, an epoxy resin and a cured product thereof. Background Art
[0002] As a semiconductor packaging material, epoxy resin is usually used for curing and sealing, among which resins formed by o-cresol novolac epoxy resin, phenol novolac curing agent and inorganic fillers such as silica are widely used for packaging. By introducing benzene rings or biphenyl structures into the epoxy resin and / or phenolic resin curing agent of the epoxy resin curing sealing material, its flame retardancy and high temperature resistance can be greatly improved. With the emerging development of new energy vehicles, consumer electronics, the Internet of Things, 5G and other industries, the performance requirements for integrated circuits and semiconductors are also developing continuously towards low size and high power with Moore's Law, which puts forward higher requirements for the high temperature and moisture resistance stability of semiconductor-related materials. How to further improve the high temperature and moisture resistance stability of epoxy resin packaging materials has become a particularly important issue. Summary of the invention
[0003] The specific embodiment of the present invention provides a phenolic resin, an epoxy resin and a cured product thereof with excellent high temperature and moisture resistance stability. The specific scheme is as follows:
[0004] A phenolic resin having a structure shown in the following formula (1):
[0005] A-(BA) m1 (1)
[0007] Where m1 is an integer from 1 to 10.
[0008] A has a structure shown in the following formula (2),
[0009]
[0010] In formula (2), R1 is a substituted or unsubstituted phenylene group, or a substituted or unsubstituted biphenylene group, n1 is an integer from 1 to 10,
[0011] The n1 in m1+1 A can be the same or different;
[0012] B has the structure shown in the following formula (3),
[0013]
[0014] In formula (3), R2 is a hydroxyl group or CX3, and X is a halogen atom.
[0015] Optionally, R2 is an ortho- or para-substituted hydroxyl group, or an ortho- or para-substituted trifluoromethyl group.
[0016] The preparation method of the above phenolic resin comprises the following steps:
[0017] 1) reacting 400 to 500 parts by weight of a benzene or biphenyl compound represented by the following formula (4) with 1000 parts by weight of phenol, and removing excess phenol under reduced pressure after the reaction is completed;
[0018] Y-CH2R1CH2-Y (4)
[0020] In formula (4), Y is a halogen atom, a hydroxyl group or a C 1-4 An alkoxy group, R1 is a substituted or unsubstituted phenylene group, or a substituted or unsubstituted biphenylene group;
[0021] 2) adding 20 to 60 parts by weight of the substituted benzaldehyde represented by formula (5) to the product of step 1) to obtain the phenolic resin by reaction,
[0022]
[0023] In formula (5), R2 is a hydroxyl group or CX3, and X is a halogen atom.
[0024] An epoxy resin having a structure shown in the following formula (6):
[0025] C-(DC) m2 (6)
[0027] Where m2 is an integer from 1 to 10.
[0028] C has the structure shown in the following formula (7),
[0029]
[0030] In formula (7), R1 is a substituted or unsubstituted phenylene group, or a substituted or unsubstituted biphenylene group, n2 is an integer from 1 to 10,
[0031] The n2 in m2+1 C can be the same or different;
[0032] D has the structure shown in the following formula (8),
[0033]
[0034] In formula (8), R2 is Or CX3, X is a halogen atom.
[0035] Optionally, R2 is an ortho- or para-substituted hydroxyl group, or an ortho- or para-substituted trifluoromethyl group.
[0036] In the above-mentioned method for preparing epoxy resin, the epoxy resin is prepared by reacting the phenolic resin with epichlorohydrin.
[0037] An epoxy resin composition comprises the phenolic resin and epoxy resin as described above.
[0038] A cured epoxy resin product, which is obtained by curing the epoxy resin composition as described above.
[0039] Optionally, the glass transition temperature of the solidified material is between 135° C. and 146° C., and the water absorption rate is between 0.4 and 0.7.
[0040] A semiconductor device, wherein the semiconductor comprises the epoxy resin cured material as described above.
[0041] The phenolic resin of the specific embodiment of the present invention has a structure shown in formula (1), and further introduces a structural unit shown in formula (3) into the structural unit shown in formula (2). The structure can further improve the high temperature and moisture stability of its epoxy resin packaging material. DETAILED DESCRIPTION
[0042] The specific embodiment of the present invention provides a phenolic resin having a structure shown in the following formula (1):
[0043] A-(BA) m1 (1)
[0045] Where m1 is an integer from 1 to 10.
[0046] A has a structure shown in the following formula (2),
[0047]
[0048] In formula (2), R1 is a substituted or unsubstituted phenylene group, or a substituted or unsubstituted biphenylene group, n1 is an integer from 1 to 10,
[0049] The n1 in m1+1 A can be the same or different;
[0050] B has the structure shown in the following formula (3),
[0051]
[0052] In formula (3), R2 is a hydroxyl group or CX3, and X is a halogen atom.
[0053] The phenolic resin of the specific embodiment of the present invention can further improve the high temperature and moisture resistance stability of the epoxy resin packaging material by introducing the benzaldehyde structure into the phenolic resin structure shown in formula (2), meet the performance requirements of integrated circuits and semiconductors, and also continue to develop towards low size and high power with Moore's Law. The benzaldehyde structure is shown in formula (3), and the benzaldehyde has a hydroxyl substituent or a CX3 substituent on the benzene ring structure. When it does not have the substituent, for example, when it is only benzaldehyde, it may not be able to effectively react with the phenolic resin shown in formula (2), and ultimately cannot effectively obtain further performance improvement.
[0054] In the phenolic resin of the specific embodiment of the present invention, in some specific embodiments, R2 in the benzaldehyde structure shown in formula (3) is a hydroxyl group. In some specific embodiments, R2 in the benzaldehyde structure shown in formula (3) is CX3. Considering the better high temperature and humidity resistance, R2 in the benzaldehyde structure shown in formula (3) is CX3.
[0055] In the phenolic resin of the specific embodiment of the present invention, in some specific embodiments, the R2 is a hydroxyl group substituted at the ortho position or the para position, and in some specific embodiments, the R2 is a trifluoromethyl group substituted at the ortho position or the para position.
[0056] In the phenolic resin of the specific embodiment of the present invention, in some specific embodiments, the R1 is an unsubstituted phenylene group, or an unsubstituted biphenylene group, that is, a phenylene group without a substituent or a biphenylene group without a substituent; in some specific embodiments, the R1 is a substituted phenylene group, or a substituted biphenylene group, that is, the phenylene or biphenylene group has a substituent on the benzene ring, such as a methyl group, an ethyl group, a hydroxyl group, a carboxyl group or an amino group, etc. Considering better high temperature resistance and moisture resistance, the R1 is an unsubstituted biphenylene group.
[0057] The phenolic resin of the specific embodiment of the present invention, in some specific embodiments, the phenolic resin has a structure shown in formula (1), wherein m1 is one of the integers from 1 to 10, for example, m1 is 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10. In some specific embodiments, the phenolic resin has a structure shown in formula (1), and m1 is multiple integers from 1 to 10, that is, the phenolic resin is a mixture of multiple integers from 1 to 10, for example, in some specific embodiments, the phenolic resin simultaneously includes the structure shown in formula (1) with m1 values of 1, 2, 3, 4, 5, 6, 7, 8, 9 and 10.
[0058] In the phenolic resin of the specific embodiment of the present invention, the n1 in m1+1 A can be the same or different. In some specific embodiments, in the structural unit A of formula (1) having the structure shown in formula (2), the n1 value in m1+1 structural units A is the same. In some specific embodiments, in the structural unit A of formula (1) having the structure shown in formula (2), the n1 value in m1+1 structural units A is different, for example, the value of n1 in one structural unit A is 1, and the value of n1 in another structural unit A is 2 or 3, and so on.
[0059] The specific embodiment of the present invention also provides a method for preparing the above phenolic resin, comprising the following steps:
[0060] 1) reacting 400 to 500 parts by weight of a benzene or biphenyl compound represented by the following formula (4) with 1000 parts by weight of phenol, and removing excess phenol under reduced pressure after the reaction is completed;
[0061] Y-CH2R1CH2-Y (4)
[0063] In formula (4), Y is a halogen atom, a hydroxyl group or a C 1-4 An alkoxy group, R1 is a substituted or unsubstituted phenylene group, or a substituted or unsubstituted biphenylene group;
[0064] 2) adding 20 to 60 parts by weight of the substituted benzaldehyde represented by formula (5) to the product of step 1) to obtain the phenolic resin by reaction,
[0065]
[0066] In formula (5), R2 is a hydroxyl group or CX3, and X is a halogen atom.
[0067] The preparation method of the phenolic resin of the specific embodiment of the present invention, in some specific embodiments, the benzene or biphenyl compound represented by formula (4) reacts with phenol under the catalysis of an acid catalyst, and the acid catalyst can be an organic acid or an inorganic acid, for example, it can be methanesulfonic acid, trifluoromethanesulfonic acid, p-toluenesulfonic acid or sulfuric acid, etc. In some specific embodiments, the reaction temperature is 20-120°C, and the reaction time is 20-20h.
[0068] In the preparation method of the phenolic resin of the specific embodiment of the present invention, in some specific embodiments, the benzene or biphenyl compound represented by formula (4) is 1,4-dichlorobenzene, 1,4-diethoxybenzene, 4,4'-bis(chloromethyl)-1,1'-biphenyl, 4,4'-bis(bromomethyl)-1,1'-biphenyl, 4,4'-bis(methoxymethyl)-1,1'-biphenyl and 4,4'-bis(ethoxymethyl)-1,1'-biphenyl, etc.
[0069] In the method for preparing phenolic resin according to the specific embodiment of the present invention, in some specific embodiments, the reaction in step 1) is carried out in the absence of a solvent, and in some specific embodiments, the reaction in step 1) is carried out in the presence of a solvent, and the solvent may be, for example, methanol, ethanol, isopropanol, methyl ethyl ketone, methyl isobutyl ketone, toluene, xylene, and the like.
[0070] In some embodiments of the method for preparing phenolic resin according to the specific embodiment of the present invention, the reaction in step 2) is carried out in the presence of a solvent, and the solvent may be, for example, aromatic hydrocarbons such as toluene and xylene, or methyl ethyl ketone, methyl isobutyl ketone (MIBK), and the like.
[0071] In the method for preparing phenolic resin according to the specific embodiment of the present invention, in some specific embodiments, the reaction temperature of step 2) is 100-150° C., and the reaction time is 5-10 hours.
[0072] The preparation method of the phenolic resin of the specific embodiment of the present invention, in formula (5), R2 is a hydroxyl group or CX3, and X is a halogen atom. Compared with the case without the substituent, such as the case of only benzaldehyde, it can effectively react with the phenolic resin shown in formula (2) to effectively obtain further improvement in performance.
[0073] The present invention is a method for preparing a phenolic resin according to an embodiment of the present invention. In some embodiments, after the reaction of step 2) is completed, the method further includes washing the product to neutrality and removing the reaction solvent.
[0074] The specific embodiment of the present invention also provides an epoxy resin having a structure shown in the following formula (6):
[0075] C-(DC) m2 (6)
[0077] Where m2 is an integer from 1 to 10.
[0078] C has the structure shown in the following formula (7),
[0079]
[0080] In formula (7), R1 is a substituted or unsubstituted phenylene group, or a substituted or unsubstituted biphenylene group, n2 is an integer from 1 to 10, and n2 in m2+1 C can be the same or different.
[0081] D has the structure shown in the following formula (8),
[0082]
[0083] In formula (8), R2 is Or CX3, X is a halogen atom.
[0084] The epoxy resin of the specific embodiment of the present invention, in some specific embodiments, the epoxy resin has a structure shown in formula (6), wherein m2 is one of the integers from 1 to 10, for example, m2 is 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10. In some specific embodiments, the epoxy resin has a structure shown in formula (6), and m2 is multiple integers from 1 to 10, that is, the epoxy resin is a mixture of multiple integers from 1 to 10, for example, in some specific embodiments, the epoxy resin simultaneously includes the structure shown in formula (6) with m2 values of 1, 2, 3, 4, 5, 6, 7, 8, 9 and 10.
[0085] In the epoxy resin of the specific embodiment of the present invention, n2 in m2+1 Cs may be the same or different. In some specific embodiments, in the structural unit C of formula (6) having the structure shown in formula (7), n2 values in m2+1 structural units C are the same. In some specific embodiments, in the structural unit C of formula (6) having the structure shown in formula (7), n2 values in m2+1 structural units C are different, for example, the value of n2 in one structural unit C is 1, and the value of n2 in another structural unit C is 2 or 3, and so on.
[0086] In the epoxy resin of the specific embodiment of the present invention, in some specific embodiments, R2 in the benzaldehyde structure shown in formula (8) is a hydroxyl group. In some specific embodiments, R2 in the benzaldehyde structure shown in formula (8) is CX3. Considering the better high temperature and humidity resistance, R2 in the benzaldehyde structure shown in formula (8) is CX3.
[0087] In the epoxy resin of the specific embodiment of the present invention, in some specific embodiments, the R2 is a hydroxyl group substituted at the ortho position or the para position, and in some specific embodiments, the R2 is a trifluoromethyl group substituted at the ortho position or the para position.
[0088] The specific embodiments of the present invention also provide a method for preparing the epoxy resin. In some specific embodiments, the epoxy resin is prepared by reacting the aforementioned phenolic resin with epichlorohydrin (C3H5XO: X is a halogen atom).
[0089] The preparation method of the epoxy resin of the specific embodiment of the present invention, in some specific embodiments, is prepared by glycidyl etherification in epihalohydrin in the presence of an alkali metal hydroxide. In some specific embodiments, the reaction temperature is 50 to 150° C., and the reaction time is 2 to 20 hours. In some specific embodiments, the reaction is carried out in a solvent, such as a solvent such as toluene or xylene.
[0090] In some specific embodiments of the epoxy resin preparation method according to the specific embodiment of the present invention, in the epoxy resin preparation method, the phenolic resin is 200 to 400 parts by weight, and the epihalohydrin is 1000 to 1200 parts by weight.
[0091] The present invention is a method for preparing a phenolic resin according to an embodiment of the present invention. In some embodiments, the method for preparing an epoxy resin further comprises the steps of washing the product to neutrality and removing excess epihalohydrin and reaction solvent.
[0092] A specific embodiment of the present invention further provides an epoxy resin composition, which includes the phenolic resin and the epoxy resin as described above.
[0093] The epoxy resin composition of the specific embodiment of the present invention, in some specific embodiments, the epoxy resin composition may also include other phenolic resins, such as phenol novolac resin, cresol novolac resin or trisphenol methane resin, etc. In some specific embodiments, the epoxy resin composition may also include other epoxy resins, such as o-cresol novolac epoxy resin, trisphenol methane epoxy resin, naphthol epoxy resin, naphthol aralkyl resin, etc.
[0094] The epoxy resin composition of the specific embodiment of the present invention, in some specific embodiments, the epoxy resin composition also includes a curing accelerator for curing the epoxy resin through the phenolic resin, as a curing accelerator, for example, organic phosphine compounds and boron salts thereof, tertiary amines, quaternary ammonium salts, imidazoles and tetraphenyl boron salts thereof, and the like, specifically triphenylphosphine.
[0095] The epoxy resin composition of the specific embodiment of the present invention, in some specific embodiments, further includes other components, such as inorganic fillers, other resin compositions, additives, and the like.
[0096] The specific embodiment of the present invention also provides an epoxy resin cured product, which is cured by the epoxy resin composition as described above. In some specific embodiments, the epoxy resin cured product has particularly excellent high temperature and moisture stability, and the glass transition temperature of the cured product is 135-146°C, and specifically, for example, it can be 135°C, 136°C, 137°C, 138°C, 139, 140°C, 141°C, 142°C, 143°C, 144, 145°C or 146°C, and the water absorption is 0.4-0.7, and specifically, for example, 0.4, 0.5, 0.6 or 0.7, etc.
[0097] A specific embodiment of the present invention also provides a semiconductor device, wherein the semiconductor includes the epoxy resin cured material as described above, and the epoxy resin is used to seal and package the semiconductor device. The semiconductor device may be, for example, an integrated circuit, a large-scale integrated circuit, a transistor, a thyristor, a diode, a solid-state imaging element, etc.
[0098] The following examples are for further illustrating the effects of the present invention, but are not limited thereto and are only for illustration and to enhance understanding.
[0099] Example
[0100] Test description:
[0101] Glass transition (Tg): Hitachi High-Tech Analytical Instruments TMA 7100 was used to increase the temperature to 200°C at a heating rate of 2°C / min, then cool the temperature to 30°C at a cooling rate of 2°C / min, and then increase the temperature to 200°C at a heating rate of 2°C / min. The glass transition temperature at the second heating was read by integration.
[0102] Water absorption rate: The sample was prepared into a disk with a diameter of 5 cm and a thickness of 4 mm. After being placed in boiling water at 100 degrees for 24 hours, its weight increase percentage (wt %) was measured.
[0103] Example 1
[0104] In a four-necked flask equipped with a stirrer, a thermometer and a condenser, 1000 parts of phenol and 1 part of concentrated sulfuric acid are placed; under stirring, 484 parts of 4,4'-biphenyl dimethyl dimethyl ether are added at 100°C, and the reactant thus obtained is reacted at 50°C for 10 hours. After the reaction is completed, all unreacted phenol is removed by reduced pressure distillation at no more than 230°C, and the temperature is lowered to below 120°C, and then 30 parts of o-hydroxybenzaldehyde and 500 parts of MIBK solvent are added, fully dissolved, and reacted at 130°C. After the reaction is completed, 500 parts of MIBK are added, and the mixture is washed with water several times until the water is neutral, and then MIBK is removed under heating vacuum conditions, and finally 702 parts of phenolic resin (P1) with a softening point of 80°C and a hydroxyl equivalent of 176q / eq are obtained.
[0105] In a four-necked flask equipped with a stirrer, a thermometer and a condenser, 353 parts of the phenolic resin (P1) prepared above, 1120 parts of epichlorohydrin and 300 parts of toluene were placed to prepare a solution, the solution was heated to 50°C, and then 82 parts of flaky sodium hydroxide (purity 99wt%) were added over a period of 90 minutes, and then the temperature was raised to 60°C for reaction for 8 hours, and then the reaction mixture was repeatedly washed with water until the washing water became neutral, and then the excess epichlorohydrin was distilled off from the organic layer under heating and reduced pressure, and then 900 parts of MIBK was added to dissolve, and the mixed solution was heated to 70°C, and 20 parts of a 20wt% sodium hydroxide aqueous solution were added to react for 2 hours, and then the reaction mixture was repeatedly washed with water until the washing water became neutral, and then MIBK was distilled off under reduced pressure at 180-200°C to obtain 466 parts of epoxy resin (E1) with an epoxy equivalent of 233 g / eq and a softening point of 70°C.
[0106] 100 parts of phenolic resin (P1), 75 parts of epoxy resin (E1) and 1 part of triphenylphosphine were mixed evenly with a stirrer, and the composition was die-cast for 200 seconds and then cured at 160°C for 2 hours and at 180°C for 6 hours to obtain a cured product. The glass transition temperature of the cured product was tested to be 138°C, and its water absorption was tested to be 0.67.
[0107] Example 2
[0108] In a four-necked flask equipped with a stirrer, a thermometer and a condenser, 1000 parts of phenol and 1 part of concentrated sulfuric acid are placed; under stirring, 484 parts of 4,4'-biphenyl dimethyl dimethyl ether are added at 100°C, and the reactant thus obtained is reacted at 50°C for 10 hours. After the reaction is completed, all unreacted phenol is removed by reduced pressure distillation at no more than 230°C, and the temperature is lowered to below 120°C, and then 50 parts of 3-(trifluoromethyl)benzaldehyde and 500 parts of MIBK solvent are added, fully dissolved, and reacted at 130°C. After the reaction is completed, 500 parts of MIBK are added, and the mixture is washed with water several times until the water is neutral, and then MIBK is removed under heating vacuum conditions, and finally 722 parts of phenolic resin (P2) with a softening point of 84°C and a hydroxyl equivalent of 212q / eq are obtained.
[0109] In a four-necked flask equipped with a stirrer, a thermometer and a condenser, 424 parts of the phenolic resin (P2) prepared above, 1120 parts of epichlorohydrin and 300 parts of toluene were placed to prepare a solution, the solution was heated to 50°C, and then 82 parts of flaky sodium hydroxide (purity 99wt%) were added over a period of 90 minutes, and then the temperature was raised to 60°C for reaction for 8 hours, and then the reaction mixture was repeatedly washed with water until the washing water became neutral, and then the excess epichlorohydrin was distilled off from the organic layer under heating and reduced pressure, and then 900 parts of MIBK was added to dissolve, and the mixed solution was heated to 70°C, and 20 parts of a 20wt% sodium hydroxide aqueous solution were added to react for 2 hours, and then the reaction mixture was repeatedly washed with water until the washing water became neutral, and then MIBK was distilled off under reduced pressure at 180-200°C to obtain 536 parts of epoxy resin (E2) with an epoxy equivalent of 267g / eq and a softening point of 75°C.
[0110] 100 parts of phenolic resin (P2), 75 parts of epoxy resin (E2) and 1 part of triphenylphosphine were mixed evenly with a stirrer, and the composition was die-cast for 200 seconds and then cured at 160°C for 2 hours and at 180°C for 6 hours to obtain a cured product. The glass transition temperature of the cured product was tested to be 145°C, and its water absorption was tested to be 0.43.
[0111] Comparative Example 1
[0112] In a four-necked flask equipped with a stirrer, a thermometer and a condenser, 1000 parts of phenol and 1 part of concentrated sulfuric acid are placed; under stirring, 484 parts of 4,4'-biphenyl dimethyl dimethyl ether are added at 100°C, and the reactant thus obtained is reacted at 50°C for 10 hours. After the reaction is completed, all unreacted phenol is removed by reduced pressure distillation at no more than 230°C, 500 parts of MIBK are added, and the mixture is washed with water several times until it is neutralized by water, and then MIBK is removed under heating vacuum conditions, and finally 663 parts of phenolic resin (P3) with a softening point of 60°C and a hydroxyl equivalent of 204q / eq are obtained.
[0113] In a four-necked flask equipped with a stirrer, a thermometer and a condenser, 408 parts of the phenolic resin (P3) prepared above, 1300 parts of epichlorohydrin and 350 parts of toluene were placed to prepare a solution, the solution was heated to 50°C, and then 82 parts of flaky sodium hydroxide (purity 99wt%) were added over a period of 90 minutes, and then the temperature was raised to 60°C for reaction for 8 hours, and then the reaction mixture was repeatedly washed with water until the washing water became neutral, and then the excess epichlorohydrin was distilled off from the organic layer under heating and reduced pressure, and then 900 parts of MIBK was added to dissolve, and the mixed solution was heated to 70°C, and 20 parts of a 20wt% sodium hydroxide aqueous solution were added to react for 2 hours, and then the reaction mixture was repeatedly washed with water until the washing water became neutral, and then MIBK was distilled off under reduced pressure at 180-200°C to obtain 518 parts of epoxy resin (E3) with an epoxy equivalent of 260 g / eq and a softening point of 50°C.
[0114] 100 parts of phenolic resin (P3), 75 parts of epoxy resin (E3) and 1 part of triphenylphosphine were mixed evenly with a stirrer, and the composition was die-cast for 200 seconds and then cured at 160°C for 2 hours and at 180°C for 6 hours to obtain a cured product. The glass transition temperature of the cured product was tested to be 130°C, and its water absorption was tested to be 0.65.
[0115] From the results of Example 1 and Comparative Example 1 above, it can be seen that after the introduction of the o-hydroxybenzaldehyde structure, the cured product of the phenolic resin having a biphenyl structure and its epoxy resin has a higher glass transition temperature, but its water absorption rate remains basically unchanged. In particular, as the results of Example 2 above show, after the introduction of the 3-(trifluoromethyl)benzaldehyde structure, the cured product of the phenolic resin having a biphenyl structure and its epoxy resin has a higher glass transition temperature and a lower water absorption rate.
[0116] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A phenolic resin, characterized in that Having the structure shown in the following formula (1), A-(B-A) m1 (1) Where m1 is an integer from 1 to 10. A has the structure shown in the following formula (2), In formula (2), R1 is a substituted or unsubstituted phenylene group, or a substituted or unsubstituted biphenylene group, n1 is an integer from 1 to 10, n1 in m1+1 A can be the same or different; B has the structure shown in the following formula (3), In formula (3), R2 is a hydroxyl group or CX3, and X is a halogen atom; The phenolic resin is a mixture of multiple integers ranging from 1 to 10 in which m1 is a value.
2. The phenolic resin according to claim 1, wherein The R2 is an ortho- or para-substituted hydroxyl group, or an ortho- or para-substituted trifluoromethyl group.
3. An epoxy resin, characterized in that Having the structure shown in the following formula (6), C-(D-C) m2 (6) Where m2 is an integer from 1 to 10, C has the structure shown in the following formula (7), In formula (7), R1 is a substituted or unsubstituted phenylene group, or a substituted or unsubstituted biphenylene group, n2 is an integer from 1 to 10, The n2 in m2+1 C can be the same or different; D has the structure shown in the following formula (8), In formula (8), R2 is or CX3, X is a halogen atom; The epoxy resin is a mixture of multiple integers ranging from 1 to 10 in which m2 is a value.
4. The epoxy resin according to claim 3, characterized in that The R2 is an ortho- or para-substituted hydroxyl group, or an ortho- or para-substituted trifluoromethyl group.
5. A method for preparing an epoxy resin as claimed in claim 3, characterized in that: The epoxy resin is prepared by reacting the phenolic resin according to claim 1 with epichlorohydrin.
6. An epoxy resin composition, characterized in that The epoxy resin composition comprises the phenolic resin according to claim 1 or 2 and the epoxy resin according to claim 3 or 4.
7. An epoxy resin cured product, characterized in that The epoxy resin cured product is formed by curing the epoxy resin composition according to claim 6.
8. A cured epoxy resin, characterized in that: The epoxy resin cured product is formed by curing the phenolic resin with the structure shown in formula (1) and the epoxy resin with the structure shown in formula (8).
9. The epoxy resin cured product according to claim 7 or 8, characterized in that The glass transition temperature of the solidified material is between 135 and 146° C., and the water absorption rate is between 0.4 and 0.
7.
10. A semiconductor device, characterized in that: The semiconductor comprises the cured epoxy resin material according to claim 7 or 8.
Citation Information
Patent Citations
Halogen-free intrinsic flame-retardant epoxy resin curing agent and preparation method thereof
CN106995526A
High-purity (fluoroalkyl)benzene derivative and process for producing the same
CN1653029A
New compound and manufacturing method thereof, and curable resin, epoxy resin composition and electronic parts device comprising the new compound
JP2006257400A
Phenolic resin composition, and epoxy resin composition containing the same, cured product of the epoxy resin composition, and semiconductor device having the cured product
JP2021105168A