Preparation method of cross-linking cationic waterborne polyurethane polyester antistatic finishing agent

Through the preparation of crosslinked cationic water-based polyurethane polyester antistatic finishing agent, the durability and feel of textile antistatic finishing agents are solved, and efficient and environmentally friendly antistatic effect is achieved, and it is suitable for a variety of textiles.

CN118955857APending Publication Date: 2024-11-15WUHAN TEXTILE UNIV +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411286996.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing textile antistatic finishing agents have shortcomings in terms of durability, feel, environmental protection and biodegradability, and it is difficult to meet the requirements of the national standard A-level static voltage half-life of less than 2s.

Method used

The preparation method of crosslinked cationic aqueous polyurethane polyester antistatic finishing agent is adopted, through diisocyanate, polyester glycol, polyether glycol, single-ended bihydroxyhydrocarbonyl polymethylsilane, cationic chain extender and crosslinked monomer, etc. The combination of components is carried out to perform prepolymerization, chain extension and quaternization reactions, and then emulsify the emulsion after forming polymers, improving the durability and feel of the finishing agent.

Benefits of technology

It significantly improves the anti-static durability of textiles, the half-life of static voltage reaches less than 2s, and the product is safe and environmentally friendly, with a good feel. It is suitable for textiles such as blankets, plush toys, and has a good market prospect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of antistatic finishing agent emulsions for synthetic fibers, and discloses a preparation method of a crosslinking cationic waterborne polyurethane polyester antistatic finishing agent. The method comprises the following steps: preparing raw materials: a polymeric monomer, a quaternization reagent, an auxiliary agent and water; dehydrating and pretreating the polymeric monomer; performing prepolymerization; chain extension; performing crosslinking; carrying out quaternization; performing emulsification; the cross-linking cationic waterborne polyurethane polyester antistatic finishing agent emulsion product is prepared. The preparation method is high in controllability and convenient in process. According to the cross-linking cationic waterborne polyurethane polyester antistatic finishing agent prepared by adopting the method, side long-chain polysiloxane is introduced into molecules, linear and branched tertiary ammonia is quaternized by adopting active oxygen silane side groups, and the active siloxane side groups can be further cross-linked with the side long-chain polysiloxane in the finishing process; the product can be widely applied to durable antistatic finishing of various chemical fiber textile products, and is good in durability; and textiles such as chemical fibers and the like can be endowed with quick-drying performance, and good market prospects are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of antistatic finishing agent emulsion technology for synthetic fibers, particularly to the field of durable antistatic finishing technology for polyester and spandex and their blended fiber textiles, specifically to a method for preparing a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent. Background Technology

[0002] In the field of antistatic finishing agents for synthetic fiber textiles, improving the conductivity of finishing agent polymers and solving the problem of antistatic durability of textiles are current research hotspots. Based on relevant reports in recent years, existing technologies can be divided into the following three categories: First, cationic polymers based on polyacrylic acid, which result in fabrics with a stiffer hand feel and reduced air permeability and tensile strength; second, nano-conductive material technology, where nanomaterials themselves contain color, causing significant changes in the color of the finished fabric, and nanomaterials also exhibit biotoxicity; and third, polyester-type cationic polymers, which have poor antistatic durability and are difficult to achieve the national standard Class A requirement of a static voltage half-life of less than 2 seconds. To address the issues of durability, hand feel, environmental friendliness, biodegradability, and widespread application of antistatic finishing agents for polyester, spandex, and their blended fiber textiles, this invention presents a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent emulsion product. This product avoids issues such as deterioration of the hand feel, color changes, and environmental toxicity associated with the finishing agent itself. Its unique aliphatic chain crosslinking structure and polysiloxane post-crosslinking structure effectively enhance the durability of the finishing agent on textiles and impart excellent smoothness, a fluffy hand feel, and elasticity to the finished fabric. The finishing process requires no high-temperature treatment, making it particularly suitable for durable antistatic finishing of synthetic fiber textiles such as blankets and plush toys. It represents an environmentally friendly, efficient, and feasible solution.

[0003] Currently, the preparation methods for durable synthetic fiber antistatic finishing agents include the following:

[0004] 1. A method for preparing a cationic polyacrylic acid polymer antistatic finishing agent, the raw materials of which include polymeric monomers, crosslinking monomers, auxiliaries and water, wherein the polymeric monomers include olefin-based cationic monomers, epoxy cationic monomers, acrylic acid and its derivatives; the crosslinking monomers are bifunctional olefin-based compounds or olefin-based epoxy compounds, olefin-based amides; and the auxiliaries are initiators.

[0005] For example, the cationic polymer preparation method disclosed in "Application of Antistatic Agent P in Polyester Fabrics" (Dyeing and Finishing Auxiliaries, 2012, No. 29) by Liu Xiaoyun, Zhong Shaofeng, Wang Xiaofang, et al., uses dimethyl diallyl ammonium chloride and acrylamide as the polymerizing and crosslinking monomers in its raw materials. The preparation method of hyperbranched cationic polyacrylamide disclosed in "Synthesis and Application Performance Study of Hyperbranched Cationic Polyacrylamide" (Master's Thesis, Suzhou University, 2014) by Chen Kun and Zhou Xiangdong includes polymerizing monomers acrylic acid, glycidyl trimethyl ammonium chloride, hyperbranched polyester, crosslinking monomers acrylamide and allyl glycidyl ether, and the initiator ammonium persulfate.

[0006] The cationic polyacrylic acid polymers prepared by the aforementioned methods exhibit strong cationic properties. Acrylamide and allyl glycidyl ether can undergo cross-linking reactions at high temperatures, resulting in a high cross-linking density in the polymer. Furthermore, the absence of long-chain soft segments in the molecule leads to reduced air permeability and tensile strength in fabrics treated with this polymer. Additionally, while the extremely high density of cationic groups in the polymer molecule can improve the antistatic properties of the treated fabric, the majority of the raw materials used are highly water-soluble monomers. After multiple washes, the antistatic properties of this finishing agent do not meet the national standard Class A requirement of a static voltage half-life of less than 2 seconds. Moreover, the high glass transition temperatures of the monomers result in a stiffer hand feel in the treated fabric, further limiting its applicability.

[0007] 2. A method for preparing a nano-conductive antistatic finishing agent, the raw materials of which include a reducing agent, a nanomaterial precursor, a binder or dispersant, etc., wherein the reducing agent includes hydrazine hydrate and ascorbic acid; the nanomaterial precursor includes graphene oxide, silver nitrate, copper nitrate, etc.; the binder is an aqueous polymer resin; and the dispersant is a surfactant.

[0008] For example, the preparation method of nano-conductive antistatic finishing agent disclosed in "Application of Graphene in Antistatic Polyester Fabrics" (Dyeing and Printing, Issue 45, late 2019) by Chen Xiaoting, Wu Shiwen, Ren Hao, et al. uses hydrazine hydrate as the reducing agent, graphene oxide as the nanomaterial, and waterborne polyurethane resin as the binder. While this method uses hydrazine hydrate to efficiently reduce graphene oxide, its high toxicity makes the preparation process extremely harmful to humans and the environment. Furthermore, although using waterborne polyurethane resin to coat conductive graphene onto the fiber surface can effectively improve the antistatic properties of the fabric, the black color of graphene itself limits the application of the finishing agent on light-colored fabrics, and the large addition of graphene carbon-based materials will cause the fabric to feel stiff.

[0009] For example, the preparation method of nano-conductive antistatic finishing agent disclosed in "Antistatic Finishing of Polyester Fabrics with Nano-Silver Particles" (Dyeing and Printing, 2017, No. 43) by Li Ke, Xu Zhizhong, Wang Ming, et al. uses ascorbic acid as the reducing agent, silver nitrate as the nanomaterial precursor, and sodium dodecyl sulfate as the dispersant in its raw materials. This method uses bio-based ascorbic acid to reduce silver nitrate to generate nano-silver ions, which are then prepared into a nano-silver dispersion using sodium dodecyl sulfate. Due to the extremely high specific surface area of ​​nanoparticles, although this property allows the finishing agent to be easily adsorbed onto the surface of polyester fibers, it also makes the nanoparticles prone to aggregation, reducing the stability of the finishing agent. Furthermore, the inherent silver-gray color of nano-silver limits the universality of the finishing agent on different fabrics, and the weak binding force between nanoparticles and polyester fibers allows them to easily penetrate human skin, accumulate in the human body, and affect human health.

[0010] 3. A method for preparing a polyester-type cationic polymeric antistatic finishing agent, the raw materials of which include polybasic acid, polyol, quaternizing reagent, auxiliary agent and water, wherein the polyol is a small triol or polyethylene glycol; the polybasic acid is a small molecule diacid; the quaternizing reagent is a small molecule halohydrocarbon; and the auxiliary agent is a polymerization catalyst.

[0011] For example, the preparation method of a polyester-type cationic polymeric antistatic finishing agent disclosed in the paper "Preparation and Application Research of Wash-Resistant Polyester Antistatic Agent" (Master's Thesis, Wuyi University, 2021) by Wang Pukai, Jia Yongtang, Yang Ming, et al. uses triethanolamine and polyester polyol as the polyol, adipic acid as the polyacid, sodium chloroacetate as the quaternizing agent, and p-toluenesulfonic acid as the polymerization catalyst. The compound prepared by this method has a polyester content of 70%, and both the degree of crosslinking and the density of the cationic quaternary ammonium salt are high. Although the finishing agent has good adsorption properties, due to the increased crosslinking density, the cationic quaternary ammonium salt is difficult to form a conductive layer. The electrostatic voltage half-life of the fabric treated with this agent only reaches the national standard C level (6.5s) after washing. Furthermore, this process involves high reaction temperature and long reaction time, and the product is easily oxidized by heat, resulting in poor environmental friendliness. Summary of the Invention

[0012] The purpose of this invention is to overcome the problem that existing antistatic finishing agents for textiles have poor antistatic durability and are difficult to achieve the national standard Class A requirement of a static voltage half-life of less than 2 seconds. This invention provides a method for preparing a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent. The finishing agent prepared by this method improves the antistatic durability of the treated fabric, and the static voltage half-life of textile products treated with this finishing agent can reach less than 2 seconds.

[0013] To achieve the above objectives, the first aspect of the present invention provides a method for preparing a crosslinked cationic waterborne polyurethane antistatic finishing agent for polyester, the method comprising the following steps:

[0014] (1) Raw material preparation: polymerizing monomers, quaternizing reagents, auxiliary agents and water; wherein, the polymerizing monomers include diisocyanate, polyester glycol, polyether glycol, mono-terminated dihydroxyalkyl polymethylsilane, cationic chain extender and crosslinking monomer; the quaternizing reagent is a halosiloxane; the auxiliary agents include polymerization catalyst and diluent;

[0015] The diisocyanate is toluene diisocyanate or isophorone diisocyanate;

[0016] The polyester glycol is a polyester glycol composed of phthalic anhydride and 1,6-hexanediol or a polyester glycol composed of dimethyl terephthalate and ethylene glycol, and the molecular weight of the polyester glycol is 1000-3000.

[0017] Polyether glycols are polyethylene glycol with a molecular weight of 2000-6000 and polyethylene glycol methyl ether with a molecular weight of 500-2000 and a single-terminated dihydroxyalkyl group.

[0018] The molecular weight of single-terminated dihydroxyalkyl polymethylsilane is 1000–2000;

[0019] The cationic chain extender is N-methyldiethanolamine or N-butyldiethanolamine;

[0020] The crosslinking monomer is a combination of cationic crosslinking monomers and nonionic crosslinking monomers, wherein the cationic crosslinking monomer is triethanolamine or N,N,N',N'-tetra(2-hydroxypentyl)ethylenediamine, and the nonionic crosslinking monomer is selected from at least one of glycerol, pentaerythritol, xylitol and sorbitol;

[0021] The quaternizing agent is at least one of bromopropyltrimethoxysilane, chloropropyltrimethoxysilane and 2-(chloromethyl)allyltrimethoxysilane;

[0022] The proportions of each component in the raw material include: based on 12 moles of diisocyanate, the moles of polyethylene glycol are 3.4–5.5, the moles of mono-dihydroxyalkyl polyethylene glycol methyl ether are 0.1–1.2, the moles of polyester glycol are 0.5–2.5, the moles of mono-dihydroxyalkyl polymethylsilane are 0.1–0.6, the moles of cationic chain extender are (10 – moles of polyether glycol – moles of polyester glycol – moles of mono-dihydroxyalkyl polymethylsilane), the moles of crosslinking monomer are 2.2–3.5 (with a molar ratio of nonionic crosslinking monomer to cationic crosslinking monomer of 1:1–3), and the moles of quaternizing agent are (0.6–1.5) × (moles of cationic chain extender + moles of cationic crosslinking monomer).

[0023] (2) Pretreatment of polyester glycol, polyether glycol and mono-terminated dihydroxyalkyl polymethylsilane: polyester glycol, polyether glycol and mono-terminated dihydroxyalkyl polymethylsilane are dehydrated under vacuum and heating conditions.

[0024] (3) Prepolymerization step: The diluent, diisocyanate, and pre-treated polyester glycol, polyether glycol, and mono-terminated dihydroxyalkyl polymethylsilane are subjected to a prepolymerization reaction under the catalysis of a polymerization catalyst to obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent prepolymer.

[0025] (4) Chain extension step: The crosslinked cationic waterborne polyurethane polyester antistatic finishing agent prepolymer is subjected to a chain extension reaction with a cationic chain extender and a diluent to obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent intermediate.

[0026] (5) Crosslinking steps: The crosslinked cationic waterborne polyurethane polyester antistatic finishing agent intermediate is reacted with cationic crosslinking monomer, nonionic crosslinking monomer and diluent to obtain crosslinked cationic waterborne polyurethane polyester antistatic finishing agent polymer.

[0027] (6) Quaternization step: The cross-linked cationic waterborne polyurethane polyester antistatic finishing agent polymer is reacted with the quaternization agent to obtain the cross-linked cationic waterborne polyurethane polyester antistatic finishing agent.

[0028] (7) Emulsification step: Mix the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent with water and emulsify it to obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent emulsion.

[0029] (8) Solvent removal: The cross-linked cationic waterborne polyurethane polyester antistatic finishing agent emulsion product is subjected to diluent removal under vacuum and heating conditions to obtain a cross-linked cationic waterborne polyurethane polyester antistatic finishing agent emulsion product with a solid content of 10-15%.

[0030] Preferably, the polymerization catalyst is stannous octoate or dibutyltin dilaurate; preferably, the amount of the polymerization catalyst is 0.01 to 0.04% by weight of the total weight of the polymerization monomers.

[0031] Preferably, the diluent is methyl ethyl ketone or acetone; preferably, the total amount of the diluent is 80-120% by weight of the total weight of the polymer monomers.

[0032] Preferably, the water is soft water with a total hardness of less than 50 ppm CaO.

[0033] Preferably, step (2) specifically includes:

[0034] (2.1) Add polyester glycol, polyether glycol and mono-terminated dihydroxyalkyl polymethylsilane into the reactor;

[0035] (2.2 Heat the material to 105-110℃ and treat it under vacuum of -0.100--0.098MPa for 120-150 min.

[0036] Preferably, step (3) specifically includes:

[0037] (3.1) Cool the material obtained in step (2.2) to 75-80℃;

[0038] (3.2) Add diisocyanate and stir continuously, control the temperature of the reaction system at 75-85℃, and stir continuously for 20-30 min;

[0039] (3.3) After the reaction in step (3.2) is completed, control the temperature of the reaction system to 85℃±5℃ and add the polymerization catalyst at a uniform rate within 10 to 15 minutes.

[0040] (3.4) After the reaction in step (3.3) is completed, the temperature of the reaction system is controlled at 85℃±5℃ and the reaction is kept at this temperature for 100~120min. During this period, diluent is added multiple times to control the viscosity of the reaction system to be less than 1000 centipoise, so as to obtain the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent prepolymer.

[0041] Preferably, step (4) specifically includes:

[0042] (4.1) Cool the material obtained in step (3.4) to below 65°C;

[0043] (4.2) Maintain the reaction temperature at 60-65℃ and add the cationic chain extender at a uniform rate over 10-30 min;

[0044] (4.3) After the reaction in step (4.2) is completed, the temperature of the reaction system is controlled at 65℃±5℃ and the reaction is kept at this temperature for 45~90min. During this period, a diluent is added to control the viscosity of the reaction system to be less than 1000 centipoise, so as to obtain the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent intermediate.

[0045] Preferably, step (5) specifically includes:

[0046] (5.1) Nonionic crosslinking monomers and cationic crosslinking monomers are added to the reaction system in step (4.3);

[0047] (5.2) Heat the reaction system to 70-80℃ and keep it at that temperature for 60-120 minutes. Add diluent multiple times during the reaction to control the reaction viscosity to less than 1000 centipoise, and obtain cross-linked cationic waterborne polyurethane polyester antistatic finishing agent polymer.

[0048] Preferably, step (6) specifically includes:

[0049] (6.1) Cool the material obtained in step (5.2) to 65-75℃;

[0050] (6.2) Add quaternizing reagent, control the reaction temperature at 65-75℃, maintain stirring reaction for 90-120 min, and obtain cross-linked cationic waterborne polyurethane polyester antistatic finishing agent.

[0051] Preferably, step (7) specifically includes:

[0052] (7.1) Keep the reaction system of step (6.2) stirred and cool it to 40-60°C, and pump the material into the emulsifier;

[0053] (7.2) Increase the stirring speed of the emulsifier, add water at 20-35°C to the emulsifier within 20-30 minutes, and stir for 15-45 minutes to obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent emulsion.

[0054] Preferably, step (8) specifically includes:

[0055] (8.1) Maintain the emulsion system of step (7.2) at 40–50°C;

[0056] (8.2) The emulsifier is kept stirring, the vacuum system and the condenser heat exchanger are turned on to recover the diluent. When there is no more diluent distillation, the vacuum system is turned off, the material is discharged and packaged.

[0057] A second aspect of the present invention provides a crosslinked cationic aqueous polyurethane polyester antistatic finishing agent prepared by the method described above.

[0058] This invention introduces long-chain polysiloxanes and long-chain polyethers into the molecules of a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent, and implements the formation of the crosslinking structure stepwise during the preparation and application processes. This specifically improves the film-forming properties and wash resistance of the finishing agent polymer on the surface of synthetic fiber textiles, thereby enhancing the antistatic durability of the treated fabric and imparting quick-drying properties to textiles such as chemical fibers, showing good market prospects. The product is safe and environmentally friendly, energy-saving and consumption-reducing, requires low dosage, and is easy to use. Compared with the prior art, this invention has the following advantages and features:

[0059] 1. The crosslinked cationic waterborne polyurethane polyester antistatic finishing agent provided by this invention has a simple structure control. It utilizes nonionic and cationic crosslinking monomers to form intramolecular crosslinks during the preparation process. It uses active oxygen silane side groups to quaternize linear and nonlinear tertiary amines. While imparting strong positive charge to the finishing agent, it can also form a second intramolecular crosslink with the side long-chain polysiloxane during the application process. This allows the finishing agent to form a film with a high crosslink density on the surface of the treated synthetic fiber fabric, which greatly improves the wash resistance of the finishing agent. Moreover, the stepwise crosslinking scheme makes the product emulsion viscosity low, which is easy to store and use.

[0060] 2. In the preparation method of the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent provided by the present invention, nonionic crosslinking agent and cationic crosslinking agent are preferably used. Through the design of the ratio of the two, the density of positive charge at the crosslinking center can be easily adjusted. The introduction of linear tertiary amine monomer can increase the electrostatic repulsion between molecules, which is beneficial to product emulsification and reduces the VOC content of the product. Moreover, the high positive charge distribution in the product is conducive to the efficient adsorption of the finishing agent on the surface of synthetic fibers, shortening the finishing time and reducing the finishing temperature. It belongs to the category of energy-saving and emission-reducing high-efficiency antistatic finishing agent.

[0061] 3. The preparation method of the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent provided by the present invention introduces flexible segments such as main chain polyether, side long chain polyether, and side long chain siloxane. This can increase the microphase separation of hydrophilic crosslinking units formed by polyether and small molecule crosslinking agents and hydrophobic crosslinking units formed by polysiloxane and active siloxane on the surface of the treated fabric in the highly crosslinked film. This reduces the influence of high crosslinking density on the fabric's hand feel and can give the fabric good elasticity and smoothness. The fabric's air permeability and tensile strength are not affected.

[0062] 4. The crosslinked cationic waterborne polyurethane polyester antistatic finishing agent provided by the present invention does not require high-temperature baking during the film-forming process, and the inorganic / organic crosslinking structure in the structure can be applied to the antistatic finishing of various high surface energy and low surface energy fibers and their blended textile products. It has wide applicability to various types of fiber textiles, strong adaptability to processing equipment, and wide application scenarios.

[0063] 5. The preparation method of the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent provided by the present invention is easy to implement and control, with a smooth process and no special requirements for production equipment; the product does not contain emulsifiers, has good emulsion stability, low solvent content, is safe and environmentally friendly, and is easy to use; the product has good application performance and a wide range of uses. Detailed Implementation

[0064] The following provides a detailed description of specific embodiments of the present invention. It should be understood that the specific embodiments described herein are for illustrative and explanatory purposes only and are not intended to limit the scope of the invention.

[0065] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0066] The preparation method of the crosslinked cationic waterborne polyurethane antistatic finishing agent for polyester provided by the present invention includes the following steps:

[0067] (1) Raw material preparation: polymerizing monomers, quaternizing reagents, auxiliary agents and water; wherein, the polymerizing monomers include diisocyanate, polyester glycol, polyether glycol, mono-terminated dihydroxyalkyl polymethylsilane, cationic chain extender and crosslinking monomer; the quaternizing reagent is a halosiloxane; the auxiliary agents include polymerization catalyst and diluent;

[0068] (2) Pretreatment of polyester glycol, polyether glycol and mono-terminated dihydroxyalkyl polymethylsilane: polyester glycol, polyether glycol and mono-terminated dihydroxyalkyl polymethylsilane are dehydrated under vacuum and heating conditions.

[0069] (3) Prepolymerization step: The diluent, diisocyanate, and pre-treated polyester glycol, polyether glycol, and mono-terminated dihydroxyalkyl polymethylsilane are subjected to a prepolymerization reaction under the catalysis of a polymerization catalyst to obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent prepolymer.

[0070] (4) Chain extension step: The crosslinked cationic waterborne polyurethane polyester antistatic finishing agent prepolymer is subjected to a chain extension reaction with a cationic chain extender and a diluent to obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent intermediate.

[0071] (5) Crosslinking steps: The crosslinked cationic waterborne polyurethane polyester antistatic finishing agent intermediate is reacted with cationic crosslinking monomer, nonionic crosslinking monomer and diluent to obtain crosslinked cationic waterborne polyurethane polyester antistatic finishing agent polymer.

[0072] (6) Quaternization step: The cross-linked cationic waterborne polyurethane polyester antistatic finishing agent polymer is reacted with the quaternization agent to obtain the cross-linked cationic waterborne polyurethane polyester antistatic finishing agent.

[0073] (7) Emulsification step: Mix the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent with water and emulsify it to obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent emulsion.

[0074] (8) Solvent removal: The cross-linked cationic waterborne polyurethane polyester antistatic finishing agent emulsion product is subjected to diluent removal under vacuum and heating conditions to obtain a cross-linked cationic waterborne polyurethane polyester antistatic finishing agent emulsion product with a solid content of 10-15%.

[0075] In this invention, the diisocyanate may be toluene diisocyanate or isophorone diisocyanate.

[0076] In this invention, the polyester diol is a polyester diol formed from phthalic anhydride and 1,6-hexanediol or a polyester diol formed from dimethyl terephthalate and ethylene glycol, and the molecular weight of the polyester diol can be 1000-3000, for example 1000, 1500, 2000, 2500 or 3000. In one embodiment, the polyester diol formed from phthalic anhydride and 1,6-hexanediol can be HF-8356.

[0077] In some embodiments, the polyether diol is polyethylene glycol with a molecular weight of 2000-6000 and a single-terminated dihydroxyalkyl polyethylene glycol methyl ether with a molecular weight of 500-2000. In this invention, the single-terminated dihydroxyalkyl polyethylene glycol methyl ether can be a nonionic polyester diol, brand name Ymer N120, with the following structural formula:

[0078]

[0079] In some embodiments, the molecular weight of the single-terminated dihydroxyalkyl polymethylsilane can be 1000-2000, for example, 1000, 1500, or 2000. In this invention, the grade of the single-terminated dihydroxyalkyl polymethylsilane can be YC2300, and its structural formula is [insert structural formula here].

[0080] In this invention, the cationic chain extender is N-methyldiethanolamine or N-butyldiethanolamine.

[0081] In this invention, the crosslinking monomer is a combination of cationic crosslinking monomer and nonionic crosslinking monomer. The cationic crosslinking monomer may be triethanolamine or N,N,N',N'-tetra(2-hydroxypentyl)ethylenediamine, and the nonionic crosslinking monomer may be selected from at least one of glycerol, pentaerythritol, xylitol and sorbitol.

[0082] In some embodiments, the quaternizing agent is at least one selected from bromopropyltrimethoxysilane, chloropropyltrimethoxysilane, and 2-(chloromethyl)allyltrimethoxysilane.

[0083] In this invention, the proportions of each component in the raw materials include: based on 12 moles of diisocyanate, the moles of polyethylene glycol are 3.4 to 5.5, the moles of mono-dihydroxyalkyl polyethylene glycol methyl ether are 0.1 to 1.2, the moles of polyester glycol are 0.5 to 2.5, the moles of mono-dihydroxyalkyl polymethylsilane are 0.1 to 0.6, the moles of cationic chain extender are (10 – the moles of polyether glycol – the moles of polyester glycol – the moles of mono-dihydroxyalkyl polymethylsilane), the moles of crosslinking monomer are 2.2 to 3.5 (with a molar ratio of nonionic crosslinking monomer to cationic crosslinking monomer of 1:1 to 3), and the moles of quaternizing agent are (0.6 to 1.5) × (the moles of cationic chain extender + the moles of cationic crosslinking monomer). When calculating the molar number of the cationic chain extender, the molar number of the polyether glycol includes the molar number of polyethylene glycol and the molar number of single-terminated dihydroxyalkyl polyethylene glycol methyl ether.

[0084] In this invention, the polymerization catalyst may be stannous octoate or dibutyltin dilaurate. In some embodiments, the amount of the polymerization catalyst may be 0.01 to 0.04% by weight of the total weight of the polymerization monomers. The total weight of the polymerization monomers is the sum of the weights of diisocyanate, polyester glycol, polyether glycol, mono-terminated dihydroxyalkyl polymethylsilane, cationic chain extender, and crosslinking monomers.

[0085] In this invention, the diluent can be methyl ethyl ketone or acetone. In some embodiments, the total amount of the diluent is 80-120% by weight of the total weight of the polymeric monomers. The total weight of the polymeric monomers is the sum of the weights of diisocyanate, polyester glycol, polyether glycol, mono-terminated dihydroxyalkyl polymethylsilane, cationic chain extender, and crosslinking monomer. In this invention, the total amount of the diluent is the sum of the amounts of diluent used in the prepolymerization step, the chain extension step, and the crosslinking step, and there is no particular limitation on the amount of diluent used in each step, as long as the viscosity of the reaction system can be controlled within a suitable range.

[0086] In this invention, the water used is soft water with a total hardness of less than 50 ppm CaO (i.e., 5 degrees). The amount of water used can be adjusted according to the solid content of the prepared product; in some embodiments, the amount of water is adjusted to allow the solid content of the product to be between 10% and 15%.

[0087] In one implementation, step (2) specifically includes:

[0088] (2.1) Add polyester glycol, polyether glycol and mono-terminated dihydroxyalkyl polymethylsilane into the reactor;

[0089] (2.2 Heat the material to 105-110℃ and treat it under vacuum of -0.100--0.098MPa for 120-150 min.

[0090] In one implementation, step (3) specifically includes:

[0091] (3.1) Cool the material obtained in step (2.2) to 75-80℃;

[0092] (3.2) Add diisocyanate and stir continuously, control the temperature of the reaction system at 75-85℃, and stir continuously for 20-30 min;

[0093] (3.3) After the reaction in step (3.2) is completed, control the temperature of the reaction system to 85℃±5℃ and add the polymerization catalyst at a uniform rate within 10 to 15 minutes.

[0094] (3.4) After the reaction in step (3.3) is completed, the temperature of the reaction system is controlled at 85℃±5℃ and the reaction is kept at this temperature for 100~120min. During this period, diluent is added multiple times to control the viscosity of the reaction system to be less than 1000 centipoise, so as to obtain the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent prepolymer.

[0095] In one implementation, step (4) specifically includes:

[0096] (4.1) Cool the material obtained in step (3.4) to below 65°C;

[0097] (4.2) Maintain the reaction temperature at 60-65℃ and add the cationic chain extender at a uniform rate over 10-30 min;

[0098] (4.3) After the reaction in step (4.2) is completed, the temperature of the reaction system is controlled at 65℃±5℃ and the reaction is kept at this temperature for 45~90min. During this period, a diluent is added to control the viscosity of the reaction system to be less than 1000 centipoise, so as to obtain the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent intermediate.

[0099] In one implementation, step (5) specifically includes:

[0100] (5.1) Nonionic crosslinking monomers and cationic crosslinking monomers are added to the reaction system in step (4.3);

[0101] (5.2) Heat the reaction system to 70-80℃ and keep it at that temperature for 60-120 minutes. Add diluent multiple times during the reaction to control the reaction viscosity to less than 1000 centipoise, and obtain cross-linked cationic waterborne polyurethane polyester antistatic finishing agent polymer.

[0102] In one implementation, step (6) specifically includes:

[0103] (6.1) Cool the material obtained in step (5.2) to 65-75℃;

[0104] (6.2) Add quaternizing reagent, control the reaction temperature at 65-75℃, maintain stirring reaction for 90-120 min, and obtain cross-linked cationic waterborne polyurethane polyester antistatic finishing agent.

[0105] In one implementation, step (7) specifically includes:

[0106] (7.1) Keep the reaction system of step (6.2) stirred and cool it to 40-60°C, and pump the material into the emulsifier;

[0107] (7.2) Increase the stirring speed of the emulsifier, add water at 20-35°C to the emulsifier within 20-30 minutes, and stir for 15-45 minutes to obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent emulsion.

[0108] In one implementation, step (8) specifically includes:

[0109] (8.1) Maintain the emulsion system of step (7.2) at 40–50°C;

[0110] (8.2) The emulsifier is kept at a medium-low speed for stirring. The vacuum system and condenser heat exchanger are turned on to recover the diluent. When there is no more diluent distillation, the vacuum system is turned off, the material is discharged, and packaged.

[0111] A second aspect of this invention provides a crosslinked cationic aqueous polyurethane antistatic finishing agent for polyester prepared by the method described above. The storage conditions for the product prepared by the method of this invention are as follows: the finished product must be stored in a cool, dry place in a sealed container.

[0112] The product prepared by the method of this invention is used for durable antistatic finishing of various chemical fiber textile products. The product is a self-emulsifying aqueous polymer emulsion that can significantly improve the hydrophilicity and antistatic properties of synthetic fiber textile products. For plush polyester textile products (such as blankets, plush toys, etc.), after being treated with commercially available products, the triboelectric voltage can be reduced to 7000V after 5 washes according to national standards, with a static voltage half-life greater than 60s. After being treated with this product, the triboelectric voltage can be reduced to below 1800V after 5 washes according to national standards, with a static voltage half-life less than 2s. In addition, this product also enhances the elasticity and hand feel of polyester long-pile blankets and polyester plush toys. Its fluffiness is tested by a Fast style meter (expressed as compressibility), and the compressibility of the fabric increases by 5% after treatment. It has good market prospects; the product is safe, environmentally friendly, and easy to use.

[0113] The following examples further illustrate the preparation method of the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent of the present invention. These examples are implemented based on the technical solution of the present invention, providing detailed implementation methods and specific operating procedures; however, the scope of protection of the present invention is not limited to the following examples.

[0114] Unless otherwise specified, the experimental methods used in the following embodiments are conventional methods in the art. Unless otherwise specified, the experimental materials used in the following embodiments are commercially available.

[0115] The following examples illustrate a method for preparing a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent.

[0116] The raw materials for this preparation method include:

[0117] 1. Polymer monomers

[0118] Diisocyanate: Isophorone diisocyanate 12.0 mol (2667.4 g);

[0119] Polyether glycol: 3.8 mol (7600.0 g) of polyethylene glycol with a molecular weight of 2000 and 1.2 mol (1200.0 g) of polyethylene glycol methyl ether with a molecular weight of 1000.

[0120] Polyester glycol: 1.6 mol (3200.0 g) of polyester glycol consisting of dimethyl terephthalate and ethylene glycol with a molecular weight of 2000, which is prepared by reacting 10 mol of dimethyl terephthalate with 11 mol of ethylene glycol;

[0121] Single-terminated dihydroxyalkyl polymethylsilane: 0.4 mol (400.0 g) of single-terminated dihydroxyalkyl polymethylsilane with a molecular weight of 1000;

[0122] Cationic chain extender: N-methyldiethanolamine 3.0 mol (357.5 g);

[0123] Cationic crosslinking monomer: 1.2 mol (110.5 g) of triethanolamine;

[0124] Nonionic crosslinking monomer: glycerol 1.2 mol (179.0 g).

[0125] 2. Quaternizing reagent

[0126] Halogenated siloxanes: 5 mol (993.6 g) of chloropropyltrimethoxysilane.

[0127] 3. Auxiliary agents

[0128] Polymerization catalyst: dibutyltin dilaurate (3.1 g);

[0129] Diluent: Methyl ethyl ketone (13000g).

[0130] 4. Water: Soft water with a total hardness of less than 50 ppm CaO (102634.7 g).

[0131] The preparation method includes the following steps:

[0132] (1) Pretreatment steps for polyester glycol, polyether glycol, and mono-dihydroxyalkyl polymethylsilane: Polyester glycol, polyether glycol, and mono-dihydroxyalkyl polymethylsilane are subjected to dehydration pretreatment under vacuum and heating conditions; this process specifically includes:

[0133] (1.1) Add polyester glycol, polyether glycol, and mono-terminated dihydroxyalkyl polymethylsilane into the reactor;

[0134] (1.2) Heat the material to 105°C and treat it under a vacuum of -0.098MPa for 120 min.

[0135] (2) Prepolymerization step: The diluent, diisocyanate, and pre-treated polyester glycol, polyether glycol, and mono-terminated dihydroxyalkyl polymethylsilane are subjected to a prepolymerization reaction under the catalysis of a polymerization catalyst to obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent prepolymer; this process specifically includes:

[0136] (2.1) Cool the material from step (1.2) to 80°C;

[0137] (2.2) Add diisocyanate and maintain stirring, control the temperature of the reaction system at 80℃, and maintain stirring for 30 min;

[0138] (2.3) Control the temperature of the reaction system to 85℃ and add the polymerization catalyst at a uniform rate within 10 min;

[0139] (2.4) Maintain the reaction system temperature at 85℃ and keep the reaction at this temperature for 120 min. Add diluent multiple times during the reaction to control the viscosity of the reaction system to be less than 1000 centipoise, and obtain crosslinked cationic waterborne polyurethane polyester antistatic finishing agent prepolymer.

[0140] (3) Chain extension step: The crosslinked cationic waterborne polyurethane polyester antistatic finishing agent prepolymer is subjected to a chain extension reaction with a cationic chain extender and a diluent to obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent intermediate; this process specifically includes:

[0141] (3.1) Cool the material from step (2.4) to below 65°C;

[0142] (3.2) Maintain the reaction temperature at 65℃ and add the cationic chain extender at a uniform rate over 30 min;

[0143] (3.3) After the reaction in step (3.2) is completed, the temperature of the reaction system is controlled at 65℃ and the reaction is kept at this temperature for 60 min. During this period, a diluent is added to control the viscosity of the reaction system to be less than 1000 centipoise, so as to obtain the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent intermediate.

[0144] (4) Crosslinking step: The crosslinked cationic waterborne polyurethane polyester antistatic finishing agent intermediate is reacted with cationic crosslinking monomers, nonionic crosslinking monomers, and diluents to obtain the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent polymer; this process specifically includes:

[0145] (4.1) Add nonionic crosslinking monomers and cationic crosslinking monomers to the reaction system in step (3.3);

[0146] (4.2) Heat the reaction system to 70℃ and keep it at that temperature for 90 min. Add diluent multiple times during the reaction to control the reaction viscosity to less than 1000 centipoise, and obtain crosslinked cationic waterborne polyurethane polyester antistatic finishing agent polymer.

[0147] (5) Quaternization step: The crosslinked cationic waterborne polyurethane polyester antistatic finishing agent polymer is reacted with a quaternization reagent to obtain the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent; this process specifically includes:

[0148] (5.1) Cool the material from step (4.2) to 65°C;

[0149] (5.2) Add quaternizing reagent, control the reaction temperature at 65℃, maintain stirring for 90 min, and obtain crosslinked cationic waterborne polyurethane polyester antistatic finishing agent.

[0150] (6) Emulsification step: The crosslinked cationic waterborne polyurethane polyester antistatic finishing agent is mixed with water and emulsified to obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent emulsion; this process specifically includes:

[0151] (6.1) Keep the reaction system of step (5.2) stirred and cooled to 60°C, and pump the material into the emulsifier;

[0152] (6.2) Increase the stirring speed of the emulsifier, add water at 25°C to the emulsifier within 20 minutes, stir for 30 minutes, and obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent emulsion.

[0153] (7) Solvent removal: The crosslinked cationic waterborne polyurethane polyester antistatic finishing agent emulsion product is subjected to diluent removal under vacuum and heating conditions to obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent emulsion product with a solid content of 14%; this process specifically includes:

[0154] (7.1) Maintain the emulsion system of step (6.2) at 50°C;

[0155] (7.2) The emulsifier is kept stirring, the vacuum system and the condenser heat exchanger are turned on to recover the diluent. When there is no more diluent distillation, the vacuum system is turned off, the material is discharged and packaged.

[0156] For polyester plush textile products (such as blankets, plush toys, etc.), after being treated with commercially available products, the triboelectric voltage can be reduced to 7000V after 5 washes according to national standards, and the static voltage half-life is greater than 60s. After being treated with the product prepared in this embodiment, the triboelectric voltage can be reduced to below 1500V after 5 washes according to national standards, and the static voltage half-life is 1.2s. In addition, this product also enhances the elasticity and hand feel of polyester long-pile blankets and polyester plush toys. Its fluffiness is tested by a Fast style meter (expressed as compressibility), and the compressibility of the fabric is increased by 5% after treatment. It has good market prospects. The product is safe, environmentally friendly, and easy to use.

[0157] Example 2

[0158] The raw materials for this preparation method include:

[0159] 1. Polymer monomers

[0160] Diisocyanate: Isophorone diisocyanate 12.0 mol (2667.4 g);

[0161] Polyether glycol: 5.0 mol (10000.0 g) of polyethylene glycol with a molecular weight of 2000 and 0.1 mol (100.0 g) of polyethylene glycol methyl ether with a molecular weight of 1000 and a single-terminated dihydroxyalkyl group.

[0162] Polyester glycol: 0.8 mol (1600.0 g) of polyester glycol with a molecular weight of 2000 phthalic anhydride and 1,6-hexanediol, which is prepared by 8 mol of phthalic anhydride and 9 mol of 1,6-hexanediol;

[0163] Single-terminated dihydroxyalkyl polymethylsilane: 0.2 mol (300.0 g) of single-terminated dihydroxyalkyl polymethylsilane with a molecular weight of 1500;

[0164] Cationic chain extender: N-methyldiethanolamine 3.9 mol (464.7 g);

[0165] Cationic crosslinking monomer: N,N,N',N'-tetra(2-hydroxypentyl)ethylenediamine 2.4 mol (358.1 g);

[0166] Nonionic crosslinking monomer: Pentaerythritol 0.8 mol (108.9 g).

[0167] 2. Quaternizing reagent

[0168] Halogenated siloxanes: 5.7 mol (1132.7 g) of chloropropyltrimethoxysilane.

[0169] 3. Auxiliary agents

[0170] Polymerization catalyst: dibutyltin dilaurate (2.4 g);

[0171] Diluent: Methyl ethyl ketone (14000.0g).

[0172] 4. Water: Soft water with a total hardness of less than 50 ppm CaO (122699.6 g).

[0173] The preparation method includes the following steps:

[0174] (1) Pretreatment steps for polyester glycol, polyether glycol, and mono-dihydroxyalkyl polymethylsilane: Polyester glycol, polyether glycol, and mono-dihydroxyalkyl polymethylsilane are subjected to dehydration pretreatment under vacuum and heating conditions; this process specifically includes:

[0175] (1.1) Add polyester glycol, polyether glycol, and mono-terminated dihydroxyalkyl polymethylsilane into the reactor;

[0176] (1.2) Heat the material to 110°C and treat it under a vacuum of -0.098MPa for 120 min.

[0177] (2) Prepolymerization step: The diluent, diisocyanate, and pre-treated polyester glycol, polyether glycol, and mono-terminated dihydroxyalkyl polymethylsilane are subjected to a prepolymerization reaction under the catalysis of a polymerization catalyst to obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent prepolymer; this process specifically includes:

[0178] (2.1) Cool the material from step (1.2) to 80°C;

[0179] (2.2) Add diisocyanate and maintain stirring, control the temperature of the reaction system at 85℃, and maintain stirring for 20 min;

[0180] (2.3) Maintain the reaction system temperature at 85℃±2℃ and add the polymerization catalyst at a uniform rate within 15 min;

[0181] (2.4) The temperature of the reaction system was controlled at 85℃±2℃, and the reaction was kept at this temperature for 120 min. During this period, diluent was added multiple times to control the viscosity of the reaction system to be less than 1000 centipoise, so as to obtain the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent prepolymer.

[0182] (3) Chain extension step: The crosslinked cationic waterborne polyurethane polyester antistatic finishing agent prepolymer is subjected to a chain extension reaction with a cationic chain extender and a diluent to obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent intermediate; this process specifically includes:

[0183] (3.1) Cool the material from step (2.4) to below 65°C;

[0184] (3.2) Maintain the reaction temperature at 65℃ and add the cationic chain extender at a uniform rate over 30 min;

[0185] (3.3) After the reaction in step (3.2) is completed, the temperature of the reaction system is controlled at 65℃±2℃ and the reaction is kept at this temperature for 45 minutes. During this period, a diluent is added to control the viscosity of the reaction system to be less than 1000 centipoise, so as to obtain the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent intermediate.

[0186] (4) Crosslinking step: The crosslinked cationic waterborne polyurethane polyester antistatic finishing agent intermediate is reacted with cationic crosslinking monomers, nonionic crosslinking monomers, and diluents to obtain the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent polymer; this process specifically includes:

[0187] (4.1) Add nonionic crosslinking monomers and cationic crosslinking monomers to the reaction system in step (3.3);

[0188] (4.2) Heat the reaction system to 70℃ and keep it at that temperature for 70 min. Add diluent multiple times during the reaction to control the reaction viscosity to less than 1000 centipoise, and obtain cross-linked cationic waterborne polyurethane polyester antistatic finishing agent polymer.

[0189] (5) Quaternization step: The crosslinked cationic waterborne polyurethane polyester antistatic finishing agent polymer is reacted with a quaternization reagent to obtain the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent; this process specifically includes:

[0190] (5.1) Cool the material from step (4.2) to 65°C;

[0191] (5.2) Add quaternizing reagent, control the reaction temperature at 70℃, maintain stirring for 120 min, and obtain crosslinked cationic waterborne polyurethane polyester antistatic finishing agent.

[0192] (6) Emulsification step: The crosslinked cationic waterborne polyurethane polyester antistatic finishing agent is mixed with water and emulsified to obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent emulsion; this process specifically includes:

[0193] (6.1) Keep the reaction system of step (5.2) stirred and cooled to 50°C, and pump the material into the emulsifier;

[0194] (6.2) Increase the stirring speed of the emulsifier, add water at 20°C to the emulsifier within 30 minutes, stir for 45 minutes, and obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent emulsion.

[0195] (7) Solvent removal: The crosslinked cationic waterborne polyurethane polyester antistatic finishing agent emulsion product is subjected to diluent removal under vacuum and heating conditions to obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent emulsion product with a solid content of 12%; this process specifically includes:

[0196] (7.1) Maintain the emulsion system of step (6.2) at 50°C;

[0197] (7.2) The emulsifier is kept stirring, the vacuum system and the condenser heat exchanger are turned on to recover the diluent. When there is no more diluent distillation, the vacuum system is turned off, the material is discharged and packaged.

[0198] For polyester plush textile products (such as blankets, plush toys, etc.), after being treated with commercially available products, the triboelectric voltage can be reduced to 7000V after 5 washes according to national standards, and the static voltage half-life is greater than 60s. After being treated with the product prepared in this embodiment, the triboelectric voltage can be reduced to below 1800V after 5 washes according to national standards, and the static voltage decay time is 0.5s. In addition, this product also enhances the elasticity and feel of polyester long-pile blankets and polyester plush toys; it has good market prospects; the product is safe, environmentally friendly, and easy to use.

[0199] Example 3

[0200] The raw materials for this preparation method include:

[0201] 1. Polymer monomers

[0202] Diisocyanate: Isophorone diisocyanate 12.0 mol (2667.4 g);

[0203] Polyether glycol: 4.0 mol (16000.0 g) of polyethylene glycol with a molecular weight of 4000 and 0.5 mol (500.0 g) of polyethylene glycol methyl ether with a molecular weight of 1000.

[0204] Polyester glycol: 2.0 mol (4000.0 g) of polyester glycol consisting of dimethyl terephthalate and ethylene glycol with a molecular weight of 2000, wherein it is prepared by 10 mol of dimethyl terephthalate and 11 mol of ethylene glycol;

[0205] Single-terminated dihydroxyalkyl polymethylsilane: 0.4 mol (400.0 g) of single-terminated dihydroxyalkyl polymethylsilane with a molecular weight of 1000;

[0206] Cationic chain extender: N-butyldiethanolamine 3.1 mol (499.8 g);

[0207] Cationic crosslinking monomer: N,N,N',N'-tetra(2-hydroxypentyl)ethylenediamine 2.1 mol (313.3 g);

[0208] Nonionic crosslinking monomer: sorbitol 0.7 mol (127.5 g).

[0209] 2. Quaternizing reagent

[0210] Halogenated siloxanes: 4.2 mol (885.1 g) of 2-(chloromethyl)allyltrimethoxysilane.

[0211] 3. Auxiliary agents

[0212] Polymerization catalyst: dibutyltin dilaurate (4.9 g);

[0213] Diluent: Methyl ethyl ketone (24000.0g).

[0214] 4. Water: Soft water with a total hardness of less than 50 ppm CaO (205453.2 g).

[0215] The preparation method includes the following steps:

[0216] (1) Pretreatment steps for polyester glycol, polyether glycol, and mono-dihydroxyalkyl polymethylsilane: Polyester glycol, polyether glycol, and mono-dihydroxyalkyl polymethylsilane are subjected to dehydration pretreatment under vacuum and heating conditions; this process specifically includes:

[0217] (1.1) Add polyester glycol, polyether glycol, and mono-terminated dihydroxyalkyl polymethylsilane into the reactor;

[0218] (1.2) Heat the material to 110°C and treat it under a vacuum of -0.099MPa for 120 min.

[0219] (2) Prepolymerization step: The diluent, diisocyanate, and pre-treated polyester glycol, polyether glycol, and mono-terminated dihydroxyalkyl polymethylsilane are subjected to a prepolymerization reaction under the catalysis of a polymerization catalyst to obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent prepolymer; this process specifically includes:

[0220] (2.1) Cool the material from step (1.2) to 78°C;

[0221] (2.2) Add diisocyanate and maintain stirring, control the temperature of the reaction system at 80℃, and maintain stirring for 30 min;

[0222] (2.3) Maintain the reaction system temperature at 85℃±1℃ and add the polymerization catalyst at a uniform rate within 15 min;

[0223] (2.4) The temperature of the reaction system was controlled at 85℃±1℃, and the reaction was kept at this temperature for 120 min. During this period, diluent was added multiple times to control the viscosity of the reaction system to be less than 1000 centipoise, so as to obtain the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent prepolymer.

[0224] (3) Chain extension step: The crosslinked cationic waterborne polyurethane polyester antistatic finishing agent prepolymer is subjected to a chain extension reaction with a cationic chain extender and a diluent to obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent intermediate; this process specifically includes:

[0225] (3.1) Cool the material from step (2.4) to below 65°C;

[0226] (3.2) Maintain the reaction temperature at 60℃ and add the cationic chain extender at a uniform rate over 30 min;

[0227] (3.3) After the reaction in step (3.2) is completed, the temperature of the reaction system is controlled at 60℃ and the reaction is kept at this temperature for 90 min. During this period, a diluent is added to control the viscosity of the reaction system to be less than 1000 centipoise, so as to obtain the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent intermediate.

[0228] (4) Crosslinking step: The crosslinked cationic waterborne polyurethane polyester antistatic finishing agent intermediate is reacted with cationic crosslinking monomers, nonionic crosslinking monomers, and diluents to obtain the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent polymer; this process specifically includes:

[0229] (4.1) Add nonionic crosslinking monomers and cationic crosslinking monomers to the reaction system in step (3.3);

[0230] (4.2) Heat the reaction system to 75℃ and keep it at that temperature for 60 min. Add diluent multiple times during the reaction to control the reaction viscosity to less than 1000 centipoise, and obtain cross-linked cationic waterborne polyurethane polyester antistatic finishing agent polymer.

[0231] (5) Quaternization step: The crosslinked cationic waterborne polyurethane polyester antistatic finishing agent polymer is reacted with a quaternization reagent to obtain the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent; this process specifically includes:

[0232] (5.1) Cool the material from step (4.2) to 70°C;

[0233] (5.2) Add quaternizing reagent, control the reaction temperature at 75℃, maintain stirring for 120 min, and obtain cross-linked cationic waterborne polyurethane polyester antistatic finishing agent.

[0234] (6) Emulsification step: The crosslinked cationic waterborne polyurethane polyester antistatic finishing agent is mixed with water and emulsified to obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent emulsion; this process specifically includes:

[0235] (6.1) Keep the reaction system of step (5.2) stirred and cooled to 40°C, and pump the material into the emulsifier;

[0236] (6.2) Increase the stirring speed of the emulsifier, add water at 20°C to the emulsifier within 30 minutes, stir for 15 minutes, and obtain the crosslinked cationic waterborne polyurethane polyester antistatic finishing agent emulsion.

[0237] (7) Solvent removal: The crosslinked cationic waterborne polyurethane polyester antistatic finishing agent emulsion product is subjected to diluent removal under vacuum and heating conditions to obtain a crosslinked cationic waterborne polyurethane polyester antistatic finishing agent emulsion product with a solid content of 11%; this process specifically includes:

[0238] (7.1) Maintain the emulsion system of step (6.2) at 45°C;

[0239] (7.2) The emulsifier is kept stirring, the vacuum system and the condenser heat exchanger are turned on to recover the diluent. When there is no more diluent distillation, the vacuum system is turned off, the material is discharged and packaged.

[0240] For polyester plush textile products (such as blankets, plush toys, etc.), after being impregnated and treated with commercially available products, the triboelectric voltage can be reduced to 7000V after 5 washes according to national standards, and the static voltage half-life is greater than 60s. After being impregnated and treated with the product prepared in this embodiment, the triboelectric voltage can be reduced to below 1400V after 5 washes according to national standards, and the static voltage decay time is 0.4s. In addition, this product also enhances the elasticity and hand feel of polyester long-pile blankets and polyester plush toys, and can impart quick-drying properties to textiles such as chemical fibers. It has good market prospects. The product is safe, environmentally friendly, and easy to use.

[0241] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A method for preparing a cross-linked cationic waterborne polyurethane polyester antistatic finishing agent, characterized in that: The method comprises the following steps: (1) Raw material preparation: polymerization monomer, quaternization agent, auxiliary agent and water; wherein the polymerization monomer includes diisocyanate, polyester diol, polyether diol, single-terminal dihydroxyl polymethylsilane, cationic chain extender and crosslinking monomer; the quaternization agent is halogenated siloxane; the auxiliary agent includes polymerization catalyst and diluent; The diisocyanate is toluene diisocyanate or isophorone diisocyanate; The polyester diol is a polyester diol of phthalic anhydride and 1,6-hexanediol or a polyester diol of dimethyl terephthalate and ethylene glycol, and the molecular weight of the polyester diol is 1000-3000; The polyether diol is polyethylene glycol with a molecular weight of 2000-6000 and a single-terminated dihydroxyl polyethylene glycol methyl ether with a molecular weight of 500-2000; The molecular weight of the single-terminal dihydroxyalkyl polymethylsilane is 1000 to 2000; The cationic chain extender is N-methyldiethanolamine or N-butyldiethanolamine; The crosslinking monomer is a combination of a cationic crosslinking monomer and a nonionic crosslinking monomer, wherein the cationic crosslinking monomer is triethanolamine or N,N,N',N'-tetrakis(2-hydroxypentyl)ethylenediamine, and the nonionic crosslinking monomer is at least one selected from glycerol, pentaerythritol, xylitol and sorbitol; The quaternizing agent is at least one of bromopropyltrimethoxysilane, chloropropyltrimethoxysilane and 2-(chloromethyl)allyltrimethoxysilane; The usage ratio of each component in the raw material includes: based on 12 moles of diisocyanate, the mole number of polyethylene glycol is 3.4-5.5, the mole number of single-terminal bishydroxyl polyethylene glycol methyl ether is 0.1-1.2, the mole number of polyester diol is 0.5-2.5, the mole number of single-terminal bishydroxyl polymethyl silane is 0.1-0.6, the mole number of cationic chain extender is (10-the mole number of polyether diol-the mole number of polyester diol-the mole number of single-terminal bishydroxyl polymethyl silane), the mole number of cross-linking monomer is 2.2-3.5 and the mole ratio of non-ionic cross-linking monomer to cationic cross-linking monomer is 1:1-3), and the mole number of quaternizing agent is (0.6-1.5)×(the mole number of cationic chain extender+the mole number of cationic cross-linking monomer); (2) Pretreatment of polyester diol, polyether diol and single-terminal bis-hydroxyalkyl polymethyl silane: pretreatment of polyester diol, polyether diol and single-terminal bis-hydroxyalkyl polymethyl silane with dehydration under vacuum and heating conditions; (3) Prepolymerization step: prepolymerizing the diluent, diisocyanate, polyester diol, polyether diol and single-terminal bishydroxyalkyl polymethylsilane after dehydration pretreatment under the catalytic action of a polymerization catalyst to obtain a cross-linked cationic waterborne polyurethane polyester antistatic finishing agent prepolymer; (4) a chain extension step: subjecting the cross-linked cationic waterborne polyurethane polyester antistatic finishing agent prepolymer to a chain extension reaction with a cationic chain extender and a diluent to obtain a cross-linked cationic waterborne polyurethane polyester antistatic finishing agent intermediate; (5) a cross-linking step: reacting the cross-linkable cationic waterborne polyurethane polyester antistatic finishing agent intermediate with a cationic cross-linking monomer, a nonionic cross-linking monomer, and a diluent to obtain a cross-linkable cationic waterborne polyurethane polyester antistatic finishing agent polymer; (6) quaternization step: reacting the cross-linked cationic waterborne polyurethane polyester antistatic finishing agent polymer with a quaternization agent to obtain a cross-linked cationic waterborne polyurethane polyester antistatic finishing agent; (7) an emulsification step of mixing and emulsifying the cross-linked cationic water-based polyurethane polyester antistatic finishing agent with water to prepare a cross-linked cationic water-based polyurethane polyester antistatic finishing agent emulsion; (8) Removal of solvent: The cross-linked cationic water-based polyurethane polyester antistatic finishing agent emulsion product is subjected to removal of diluent under vacuum and heating conditions to obtain a cross-linked cationic water-based polyurethane polyester antistatic finishing agent emulsion product having a solid content of 10 to 15%.

2. The method according to claim 1, characterized in that The polymerization catalyst is stannous octoate or dibutyltin dilaurate. Preferably, the amount of the polymerization catalyst is 0.01 to 0.04 weight % of the total weight of the polymerization monomers; The diluent is methyl ethyl ketone or acetone. Preferably, the total amount of the diluent is 80 to 120 weight % of the total weight of the polymerized monomers; The water is soft water with a total hardness of less than 50 ppm CaO.

3. The method according to claim 1 or 2, characterized in that: The process of step (2) specifically includes: (2.1) putting polyester diol, polyether diol and single-terminal bishydroxyalkyl polymethylsilane into a reactor; (2.2 Heat the material to 105-110°C and treat it under a vacuum of -0.100-0.098 MPa for 120-150 min.

4. The method according to claim 1 or 2, characterized in that: The process of step (3) specifically includes: (3.1) Cooling the material obtained in step (2.2) to 75-80°C; (3.2) Add diisocyanate and continue stirring, control the temperature of the reaction system to 75-85°C, and continue stirring for 20-30 minutes; (3.3) After the reaction of step (3.2) is completed, the temperature of the reaction system is controlled to 85°C ± 5°C, and the polymerization catalyst is added at a uniform rate within 10 to 15 minutes; (3.4) After the reaction of step (3.3) is completed, the temperature of the reaction system is controlled to 85°C ± 5°C, and the reaction is kept warm for 100 to 120 minutes. During this period, a diluent is added in multiple times to control the viscosity of the reaction system to less than 1000 centipoise, thereby obtaining a cross-linked cationic water-based polyurethane polyester antistatic finishing agent prepolymer.

5. The method according to claim 1 or 2, characterized in that: The process of step (4) specifically includes: (4.1) Cooling the material obtained in step (3.4) to below 65°C; (4.2) maintaining the reaction temperature at 60-65°C, adding the cationic chain extender at a uniform rate within 10-30 minutes; (4.3) After the reaction of step (4.2) is completed, the temperature of the reaction system is controlled to 65°C ± 5°C, and the reaction is kept warm for 45 to 90 minutes. During this period, a diluent is added to control the viscosity of the reaction system to less than 1000 centipoise, thereby obtaining a cross-linked cationic water-based polyurethane polyester antistatic finishing agent intermediate.

6. The method according to claim 1 or 2, characterized in that: The process of step (5) specifically includes: (5.1) adding nonionic crosslinking monomers and cationic crosslinking monomers into the reaction system of step (4.3); (5.2) Raise the temperature of the reaction system and control it to 70-80°C, keep the temperature and react for 60-120 minutes, during which time add a diluent several times to control the reaction viscosity to less than 1000 centipoise, and obtain a cross-linked cationic water-based polyurethane polyester antistatic finishing agent polymer.

7. The method according to claim 1 or 2, characterized in that: The process of step (6) specifically includes: (6.1) Cooling the material obtained in step (5.2) to 65-75°C; (6.2) Add a quaternary ammonium reagent, control the reaction temperature to 65-75°C, maintain stirring for 90-120 minutes, and obtain a cross-linked cationic water-based polyurethane polyester antistatic finishing agent.

8. The method according to claim 1 or 2, characterized in that: The process of step (7) specifically includes: (7.1) The reaction system of step (6.2) is stirred and cooled to 40-60°C, and the material is pumped into an emulsifier; (7.2) Increase the stirring speed of the emulsifier, add water at 20 to 35°C into the emulsifier within 20 to 30 minutes, and stir for 15 to 45 minutes to obtain a cross-linked cationic water-based polyurethane polyester antistatic finishing agent emulsion.

9. The method according to claim 1 or 2, characterized in that: The process of step (8) specifically includes: (8.1) maintaining the emulsified system of step (7.2) at 40-50°C; (8.2) The emulsifier maintains stirring, opens the vacuum system and condensation heat exchanger, recovers the diluent, and when no diluent is distilled out, closes the vacuum system, discharges the material, and packages it.

10. A cross-linked cationic waterborne polyurethane polyester antistatic finishing agent prepared by the method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Crease-resistant antistatic polyester fabric and preparation method thereof

    CN119372927A