Porous polyurethane composite material as well as preparation method and application thereof

By preparing porous polyurethane composite materials, using pore-generating agent to form a combination of different pore density structures and conductive carbon materials, the problem of insufficient sensitivity and stability of polyurethane flexible substrate materials is solved, the sensitivity and stability are improved, and direction identification is provided and excellent durability.

CN118955992APending Publication Date: 2024-11-15WUYI UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410919566.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing polyurethane flexible substrate materials have low sensitivity and poor stability, making it difficult to meet the needs of large-scale commercial production.

Method used

Using the preparation method of porous polyurethane composite materials, a double-layer film is formed by mixing polyurethane, organic solvent, curing agent and pore-generating agent, and mixed with a conductive carbon material solution under vacuum conditions to remove pore-generating agent to improve the pore density structure. , a porous polyurethane composite material with direction recognition ability is formed.

Benefits of technology

It significantly improves the sensitivity and stability of porous polyurethane composites, can show different sensitivity responses under different force directions, is suitable for direction identification, and maintains good resistance change rate and durability after multiple stretches.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955992A_ABST
    Figure CN118955992A_ABST
Patent Text Reader

Abstract

The invention discloses a porous polyurethane composite material as well as a preparation method and application thereof. The method comprises the following steps: S1, mixing polyurethane, an organic solvent, a curing agent and a pore-foaming agent I to obtain slurry I; mixing polyurethane, an organic solvent, a curing agent and a pore-foaming agent II to obtain slurry II; s2, respectively leveling the slurry I and the slurry II to form films; a polyurethane film I and a polyurethane film II are obtained; s3, enabling two surfaces of the polyurethane film I and the polyurethane film II to be in contact, drying and adhering to obtain a double-layer film; and S4, removing the pore-foaming agent to obtain a porous double-layer membrane, mixing the porous double-layer membrane and the conductive carbon material solution under a vacuum condition, and drying to obtain the porous double-layer membrane. The mesh number of the pore-foaming agent I is 20-50, and the mesh number of the pore-foaming agent II is 55-80. According to the double-layer porous polyurethane composite material prepared by the preparation method disclosed by the invention, the sensitivity and the stability can be greatly improved. And the direction of the force can be identified.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a porous polyurethane composite material and a preparation method and application thereof. Background Art

[0002] In recent years, with the development of health monitoring, sports monitoring, entertainment technology and other fields, people have put forward higher requirements for flexible pressure sensors. The selection of sensitive materials in flexible pressure sensors and the design of their structures have become research hotspots. Polyurethane strain-type flexible sensors have the remarkable characteristics of light weight, large strain range, wide sources, low price and simple device manufacturing.

[0003] However, the currently used polyurethane flexible substrates have the defects of low sensitivity and poor stability, and are expensive and unsuitable for large-scale commercial production.

[0004] Therefore, it is necessary to develop a new method for preparing porous polyurethane composites. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the first aspect of the present invention provides a method for preparing a porous polyurethane composite material, which can effectively improve the sensitivity and stability of the porous polyurethane composite material.

[0006] The second aspect of the present invention also provides a porous polyurethane composite material.

[0007] The third aspect of the present invention also provides a flexible sensor.

[0008] A method for preparing a porous polyurethane composite material according to an embodiment of the first aspect of the present invention comprises the following steps:

[0009] S1, mixing polyurethane, organic solvent, curing agent and porogen I to obtain slurry I; mixing polyurethane, organic solvent, curing agent and porogen II to obtain slurry II;

[0010] S2, leveling slurry I and slurry II respectively to form films to obtain polyurethane film I and polyurethane film II;

[0011] S3, contacting the two surfaces of the polyurethane film I and the polyurethane film II, drying and adhering them to obtain a double-layer film;

[0012] S4, removing the porogen I and porogen II in the double-layer membrane to obtain a porous double-layer membrane, mixing the porous double-layer membrane and the conductive carbon material solution under vacuum conditions, and drying;

[0013] The mesh number of the porogen I is 20-50 meshes, and the mesh number of the porogen II is 55-80 meshes.

[0014] The method for preparing the porous polyurethane composite material according to the embodiment of the present invention has at least the following beneficial effects:

[0015] The double-layer porous polyurethane composite material prepared by the preparation method of the present invention can greatly improve sensitivity and stability. In addition, the present invention selects different mesh sizes of porogen I and porogen II to form two layers of different pore density structures, so the direction of the force can be identified.

[0016] Furthermore, when the porous polyurethane composite material of the present invention is used in a pressure sensor, it can be used for direction identification, for example, the sensitivity shown when pressure is applied to the left and the right is different. Therefore, the direction can be determined according to the different sensitivity responses.

[0017] According to some embodiments of the present invention, the porogen I and the porogen II are independently selected from at least one of sodium chloride, white sugar, and monosodium glutamate.

[0018] According to some embodiments of the present invention, based on the total mass of the slurry I, the content of the porogen I is 70% to 75%.

[0019] According to some embodiments of the present invention, the content of the porogen II is 70% to 75% based on the total mass of the slurry II.

[0020] According to some embodiments of the present invention, the content of the polyurethane is 20-25% calculated based on the total mass of the slurry I.

[0021] According to some embodiments of the present invention, the content of the polyurethane is 20-25% based on the total mass of the slurry II.

[0022] According to some embodiments of the present invention, the organic solvent is selected from N,N-dimethylacetamide and / or N,N-dimethylformamide.

[0023] According to some embodiments of the present invention, the conductive carbon material in the conductive carbon material solution is selected from at least one of carbon nanotubes, carbon black or carbon nanosheets.

[0024] According to some embodiments of the present invention, the mesh size of the porogen I is about 45 meshes, and the mesh size of the porogen II is about 60 meshes. Therefore, when the mesh sizes of the porogen I and the porogen II are the above values, higher sensitivity and stability are achieved.

[0025] According to some embodiments of the present invention, the curing agent is selected from isocyanate curing agents.

[0026] According to some embodiments of the present invention, in step S4, the steps of removing the porogen I and the porogen II in the double-layer film are as follows:

[0027] The double-layer membrane is immersed in circulating water at 60-90° C. and ultrasonically assisted to be washed several times.

[0028] A porous polyurethane composite material provided according to an embodiment of the second aspect of the present invention is prepared by the preparation method described in the first aspect of the present invention.

[0029] The third aspect of the present invention provides a flexible sensor, wherein the base material of the flexible sensor is the porous polyurethane composite material described in the second aspect of the present invention.

[0030] If there is no special explanation, the actual meaning of “about” in the present invention is that the error is allowed to be within the range of ±2%, for example, about 45 is actually 45±2%×100.

[0031] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0033] Figure 1 is a schematic diagram of a flow chart of Embodiment 1 of the present invention;

[0034] Figure 2 is a sensitivity result diagram of an embodiment of the present invention when the stretching rate is 12.5%;

[0035] Figure 3 is a sensitivity result diagram of an embodiment of the present invention when the stretching rate is 25%;

[0036] Figure 4 is a bending test experimental diagram of the porous polyurethane composite material according to an embodiment of the present invention;

[0037] Figure 5 This is a stability test diagram of the porous polyurethane composite material of Example 1 of the present invention. DETAILED DESCRIPTION

[0038] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.

[0039] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0040] Example 1

[0041] This example provides a method for preparing a porous polyurethane composite material. The preparation process diagram is shown in Figure 1 As shown, the following steps are included:

[0042] S1, weigh 42g of salt (NaCl) particles (60 mesh), 12g of polyurethane (HK-3010), 1g of N,N-dimethylacetamide (DMA) and 1g of curing agent (HK-825), stir at high speed for 3min, and obtain slurry I after stirring evenly;

[0043] Weigh 42 g of salt (NaCl) particles (45 mesh), 12 g of polyurethane (HK-3010), 1 g of N,N-dimethylacetamide (DMA) and 1 g of curing agent (HK-825), stir at high speed for 3 min, and obtain slurry II after stirring evenly;

[0044] S2. Leveling and film formation: Pour slurry I onto a polyester film that has been cut in half (one side is pre-laid flat on a grooved plate with a certain thickness), use a medicine spoon to assist in the pouring process, cover the mixture with the other side of a sealed bag, and cover it with a large glass plate; place a 2 kg weight on the glass plate to apply pressure to prepare polyurethane film I; similarly, prepare polyurethane film II.

[0045] S3, transfer to an oven at 80°C, pre-bake for 4 minutes, take out two films at the same time and tear off the polyester film on the upper surface gently from an angle with uniform force. After tearing off the film on the upper surface, continue to put the remaining part into the oven and bake for 4 minutes. Then tear off the film on the lower surface, and stick the lower surfaces of the two together. Due to the action of gravity, the polyurethane at the interface of the bonding flows, achieving stable adhesion between the films, and continue baking for 4 hours to obtain a double-layer film.

[0046] S4. Removal of salt particles: Immerse the dried double-layer membrane in 80°C circulating water for ultrasonic-assisted washing, with each ultrasonic treatment lasting 30 minutes and circulating for about three times; use a vacuum-assisted impregnation method to adsorb CNT dispersion (concentration of 0.25%; 500 mL) inside the porous double-layer membrane, and prepare it after washing and drying.

[0047] Example 2

[0048] This example provides a method for preparing a porous polyurethane composite material, comprising the following steps:

[0049] S1, weigh 42g of salt (NaCl) particles (60 mesh), 12g of polyurethane (HK-3010), 1g of N,N-dimethylacetamide (DMA) and 1g of curing agent (HK-825), stir at high speed for 3min, and obtain slurry I after stirring evenly;

[0050] Weigh 42 g of salt (NaCl) particles (30 mesh), 12 g of polyurethane (HK-3010), 1 g of N,N-dimethylacetamide (DMA) and 1 g of curing agent (HK-825), stir at high speed for 3 min, and obtain slurry II after stirring evenly;

[0051] S2. Leveling and film formation: Pour slurry I onto a polyester film that has been cut in half (one side is pre-laid flat on a grooved plate with a certain thickness), use a medicine spoon to assist in the pouring process, cover the mixture with the other side of a sealed bag, and cover it with a large glass plate; place a 2 kg weight on the glass plate to apply pressure to prepare polyurethane film I; similarly, prepare polyurethane film II.

[0052] S3, transfer to an oven at 80°C, pre-bake for 4 minutes, take out two films at the same time and tear off the polyester film on the upper surface gently from an angle with uniform force. After tearing off the film on the upper surface, continue to put the remaining part into the oven and bake for 4 minutes. Then tear off the film on the lower surface, and stick the lower surfaces of the two together. Due to the action of gravity, the polyurethane at the interface of the bonding flows, achieving stable adhesion between the films, and continue baking for 4 hours to obtain a double-layer film.

[0053] S4. Removal of salt particles: Immerse the dried double-layer membrane in 80°C circulating water for ultrasonic-assisted washing, with each ultrasonic treatment lasting 30 minutes and circulating for about three times; use a vacuum-assisted impregnation method to adsorb CNT dispersion (concentration of 0.25%; 500 mL) inside the porous double-layer membrane, and prepare it after washing and drying.

[0054] Comparative Example 1

[0055] This example provides a method for preparing a porous polyurethane composite material, comprising the following steps:

[0056] S1, weigh 42g of salt (NaCl) particles (45 mesh), 12g of polyurethane (HK-3010), 1g of N,N-dimethylacetamide (DMA) and 1g of curing agent (HK-825), stir at high speed for 3min, and obtain slurry I after stirring evenly;

[0057] Weigh 42 g of salt (NaCl) particles (30 mesh), 12 g of polyurethane (HK-3010), 1 g of N,N-dimethylacetamide (DMA) and 1 g of curing agent (HK-825), stir at high speed for 3 min, and obtain slurry II after stirring evenly;

[0058] S2. Leveling and film formation: Pour slurry I onto a polyester film that has been cut in half (one side is pre-laid flat on a grooved plate with a certain thickness), use a medicine spoon to assist in the pouring process, cover the mixture with the other side of a sealed bag, and cover it with a large glass plate; place a 2 kg weight on the glass plate to apply pressure to prepare polyurethane film I; similarly, prepare polyurethane film II.

[0059] S3, transfer to an oven at 80°C, pre-bake for 4 minutes, take out two films at the same time and tear off the polyester film on the upper surface gently from an angle with uniform force. After tearing off the film on the upper surface, continue to put the remaining part into the oven and bake for 4 minutes. Then tear off the film on the lower surface, and stick the lower surfaces of the two together. Due to the action of gravity, the polyurethane at the interface of the bonding flows, achieving stable adhesion between the films, and continue baking for 4 hours to obtain a double-layer film.

[0060] S4. Removal of salt particles: Immerse the dried double-layer membrane in 80°C circulating water for ultrasonic-assisted washing, with each ultrasonic treatment lasting 30 minutes and circulating for about three times; use a vacuum-assisted impregnation method to adsorb CNT dispersion (concentration of 0.25%; 500 mL) inside the porous double-layer membrane, and prepare it after washing and drying.

[0061] Comparative Example 2

[0062] Comparative Example 2 provides a method for preparing a porous polyurethane composite material, the steps are as follows:

[0063] S1, weigh 42g of salt (NaCl) particles (60 mesh), 12g of polyurethane (HK-3010), 1g of N,N-dimethylacetamide (DMA) and 1g of curing agent (HK-825), stir at high speed for 3min, and obtain slurry I after stirring evenly;

[0064] S2, pouring the slurry I onto a polyester film that has been cut into two halves (one side is pre-laid flat on a groove plate with a certain thickness), using a medicine spoon to assist in the pouring process, covering the mixture with a sealed bag on the other side, and covering it with a large glass plate; placing a 2 kg weight on the glass plate to apply pressure to prepare a polyurethane film I;

[0065] S3. Removal of salt particles: The dried double-layer membrane is immersed in 80°C circulating water for ultrasonic-assisted washing, with each ultrasonic washing lasting 30 minutes and circulating for about three times; the CNT dispersion (concentration of 0.25%; 500 mL) is adsorbed inside the porous double-layer membrane by vacuum-assisted impregnation, and the membrane is prepared after washing and drying.

[0066] Performance Testing

[0067] Sensitivity test

[0068] The porous polyurethane composite materials of Examples 1 to 2 of the present invention and Comparative Examples 1 to 2 were subjected to tensile tests using a flexible electronic tester, and the sensitivity was calculated. The tensile parameters were set as follows: tensile speed 2 mm / s, tensile elongation 12.5% ​​and 25%, and tensile times 20 times.

[0069] This experiment uses the strain coefficient (GF) of the strain-type flexible sensor to represent the sensitivity coefficient of the asymmetric polyurethane pressure sensor. The calculation formula of GF is as follows:

[0070] GF=(ΔR / R0) / ε

[0071] in:

[0072] GF is the sensing coefficient, also known as sensitivity;

[0073] ΔR is the change in resistance of the flexible strain sensor after deformation, that is, R-R0, where R is the resistance value after deformation and R0 is the initial resistance value.

[0074] The test results are as follows Figure 2 and Figure 3 As shown, from Figure 2 and Figure 3 According to the results, the sensitivities of the porous polyurethane composite materials of Examples 1 and 2 of the present invention are 1.42651 and 0.6912, respectively, when the elongation is 12.5%. The sensitivity of Comparative Example 1 is 0.4036; the sensitivity of Comparative Example 2 is 0.49927; when the tensile elongation is 25%, the sensitivities of Example 1 and Example 2 are 1.63763 and 1.21532, respectively. The sensitivity of Comparative Example 1 is 0.77384; the sensitivity of Comparative Example 2 is 1.05552. The double-layer porous polyurethane composite material prepared by the present invention may increase in sensitivity as the degree of tensile strain increases, and the conductive circuit of the carbon nanotubes is more damaged.

[0075] Bending test

[0076] The test connection method is the same as the flexible tensile test. This test is to bend from the outside to the inside. Because the hole density on both sides is different, it is necessary to analyze the test results obtained by bending the same membrane with different hole densities as the outside and bending to the inside to simulate the sample bending in different directions. Finally, the direction can be identified according to its resistance change rate. The resistance change rate fed back by the outside of different mesh numbers is different.

[0077] The results are as follows Figure 4 As shown, from Figure 4 It can be seen that the inside and outside show different resistance change rates, so the direction recognition can be determined by the resistance change rate.

[0078] Stability test

[0079] Sensor assembly: Copper foil is attached to the upper and lower sides of the porous polyurethane composite material of Example 1 of the present invention, the gap is filled with conductive silver paste, and the resistance can be measured using a digital source meter.

[0080] The results are as follows Figure 5 As shown, the resistance change was recorded by stretching it 400 times using a flexible electronic tester. After testing, it was found that the resistance basically did not change, thus proving its excellent stability.

[0081] In addition, under the conditions of stretching length of 4mm and stretching rate of 2mm / s, its resistance decreases slightly and still maintains a stable fluctuation, that is, the resistance fluctuation range is similar, maintaining good resistance change rate stability and sensitivity stability. Therefore, the sensor shows high durability and stability, and can maintain its performance after multiple stretching, and has a long service life.

[0082] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. A method for preparing a porous polyurethane composite material, characterized in that: The steps include: S1, mixing polyurethane, organic solvent, curing agent and porogen I to obtain slurry I; mixing polyurethane, organic solvent, curing agent and porogen II to obtain slurry II; S2, leveling slurry I and slurry II into films respectively; Obtaining polyurethane film I and polyurethane film II; S3, contacting the two surfaces of the polyurethane film I and the polyurethane film II, drying and adhering them to obtain a double-layer film; S4, removing the porogen I and porogen II in the double-layer membrane to obtain a porous double-layer membrane, mixing the porous double-layer membrane and the conductive carbon material solution under vacuum conditions, and drying; The mesh number of the porogen I is 20-50 meshes, and the mesh number of the porogen II is 55-80 meshes.

2. The method for preparing the porous polyurethane composite material according to claim 1, characterized in that: The pore-forming agent I and pore-forming agent II are independently selected from at least one of sodium chloride, white sugar and monosodium glutamate.

3. The method for preparing the porous polyurethane composite material according to claim 1, characterized in that: Calculated based on the total mass of the slurry I, the content of the porogen I is 70% to 75%.

4. The method for preparing the porous polyurethane composite material according to claim 1, characterized in that: Calculated based on the total mass of slurry II, the content of the porogen II is 70% to 75%.

5. The method for preparing the porous polyurethane composite material according to claim 1, characterized in that: Calculated based on the total mass of slurry I, the content of the polyurethane is 20-25%.

6. The method for preparing the porous polyurethane composite material according to claim 1, characterized in that: Calculated based on the total mass of slurry II, the content of the polyurethane is 20-25%.

7. The method for preparing a porous polyurethane composite material according to claim 1, characterized in that: The organic solvent is selected from N,N-dimethylacetamide and / or N,N-dimethylformamide.

8. The method for preparing a porous polyurethane composite material according to claim 1, characterized in that: The conductive carbon material in the conductive carbon material solution is selected from at least one of carbon nanotubes, carbon black or carbon nanosheets.

9. A porous polyurethane composite material, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 8.

10. A flexible sensor, characterized in that: The base material of the flexible sensor is the porous polyurethane composite material according to claim 9.

Citation Information

Cited By

  • Super-soft waterborne polyurethane synthetic leather and preparation method thereof

    CN120649310A