Organic solvent resistant PE pipe and preparation method thereof
By adding polytetrafluoroethylene and polyimide chopped fibers to the PE pipe and forming a fluorine-containing silicone coating on the surface, the problem of PE pipe swelling in organic solvents is solved, and the resistance to organic solvents and machinery is improved Performance extends service life.
Patent Information
- Application Number
- CN202411043139.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
Existing PE pipes are prone to swelling or dissolving after being exposed to organic solvents for a long time, resulting in a decline in mechanical properties and even a burst or cracking phenomenon.
Polytetrafluoroethylene and polyimide chopped fibers are used as the main raw materials, and a protective coating of fluorine-containing silicone coating is formed on the surface of the pipe. The fluorosilicone rubber layer is formed through hydrogen siliconization reaction to prevent the infiltration of organic solvents and improve the The pipes are organic solvent resistance and low swelling.
It effectively improves the organic solvent resistance and low swelling of PE pipes, enhances the rigidity and impact strength of the pipes, extends the service life, maintains the appearance, and reduces the corrosion and dissolution of the pipes by solvents.
Smart Images

Figure CN118956036A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of plastic pipes, and in particular to an organic solvent-resistant PE pipe and a preparation method thereof. Background Art
[0002] With the rapid development of plastic pipes in my country, the quality of pipes is also constantly improving. Among them, PE pipes have been widely used in building water supply and drainage, building heating, gas pipes, electrical and telecommunications protection pipe sleeves, industrial or agricultural pipes, etc. due to their own advantages such as crack resistance, low temperature resistance, resistance to corrosion by various chemicals, and good flexibility. It is one of the most widely used plastic pipes at present.
[0003] At present, most of the common PE pipes on the market use high-density polyethylene as the base material and are prepared by extrusion molding with a single structure. Although polyethylene is an inert material with a certain degree of chemical corrosion resistance, due to the special molecular structure of high-density polyethylene, the polyethylene in the PE pipe will swell after long-term contact with organic solvents such as aliphatic hydrocarbons, aromatic hydrocarbons and halogenated hydrocarbons. If the temperature exceeds 70°C, polyethylene will even dissolve in small amounts in organic solvents such as toluene and amyl acetate. This swelling or dissolution phenomenon further accelerates the structural aging of the PE pipe, resulting in a decrease in the mechanical properties of the PE pipe. If the compressive strength of the PE pipe drops below the internal or external pressure, it may even burst or crack. Summary of the invention
[0004] In order to further improve the organic solvent resistance of PE pipes and reduce the phenomenon of PE pipes swelling or dissolving in organic solvents, the present application provides an organic solvent-resistant PE pipe and a preparation method thereof.
[0005] In the first aspect, the present application provides an organic solvent-resistant PE pipe adopting the following technical solution: A PE pipe resistant to organic solvents, comprising a pipe body and a protective coating disposed on the inner and outer surfaces of the pipe body, wherein the protective coating is formed by coating and curing a fluorine-containing organic silicon coating on the surface of the pipe body, and the pipe body is made of the following raw materials in parts by weight: High-density polyethylene: 100 parts; Polytetrafluoroethylene: 4-8 parts; Polyimide chopped fibers: 2-4 parts; Compatibilizer: 2-3 parts; Masterbatch: 3-5 parts; Reinforcing filler: 4-5 parts; Antioxidants: 1.5-1.8 parts; Wherein, the length of the polyimide chopped fibers ranges from 6 to 10 mm.
[0006] By adopting the above technical scheme, by adding polytetrafluoroethylene and polyimide chopped fibers, and then combining with a layer of protective coating formed by curing fluorinated silicone coating, the organic solvent tolerance and low swelling property of PE pipes can be effectively improved. At the same time, polyimide chopped fibers can also be used as reinforcing fibers to further reinforce the main body of the pipe, which can not only improve the rigidity and impact strength of the main body of the pipe, improve the comprehensive mechanical properties of the PE pipe, but also reduce the creep of the PE pipe under long-term load, improve the anti-seepage effect of the main body of the pipe, and improve the hydrostatic strength of the PE pipe.
[0007] Secondly, the protective coating can not only block organic solvents from penetrating into the pipe body, reduce the swelling of the pipe body, and improve the organic solvent resistance of the PE pipe, but also the protective coating can protect the pipe body as a whole, which can prevent the pipe body from being affected by the outside world and causing corrosion, aging, rupture and other problems, which is beneficial to increasing the service life of the PE pipe, but also prevent the polyimide chopped fibers in the pipe body from being exposed due to external factors such as pipe aging and damage, which is beneficial to maintaining the appearance of the PE pipe for a long time.
[0008] Optionally, the fluorine-containing silicone coating comprises the following raw materials mixed in parts by weight: Vinyl-terminated fluorosilicone oil: 30-35 parts; End-hydrogenated silicone oil: 1-1.5 parts; Chloroplatinic acid: 0.12-0.15 parts; Rutile titanium dioxide: 0.3-0.45 parts.
[0009] By adopting the above technical solution, the vinyl-terminated fluorosilicone oil and the hydrogen-terminated silicone oil can undergo a hydrosilicification reaction under the catalysis of chloroplatinic acid. During the reaction, the hydrogen atoms of the hydrogen-terminated silicone oil will undergo an addition reaction with the vinyl of the vinyl-terminated fluorosilicone oil, thereby forming a protective coating of fluorine-containing silicone rubber on the inner and outer surfaces of the pipe body, which can effectively block the penetration of organic solvents into the pipe body, thereby helping to reduce the swelling of the pipe body and improve the organic solvent resistance of the PE pipe. In addition, the fluorine-containing silicone rubber also has excellent resistance to organic solvents, which can also reduce the erosion and swelling of the protective coating by organic solvents, which is conducive to the protective coating protecting the pipe body for a long time.
[0010] Optionally, the vinyl mass fraction of the vinyl-terminated fluorosilicone oil is 1.2%-1.5%, and the viscosity of the vinyl-terminated fluorosilicone oil is 300-500mm 2 / s, and the mass fraction of active hydrogen in the terminal hydrogen-containing silicone oil is 0.4%-0.6%.
[0011] By adopting the above technical solution, when the vinyl mass fraction of the end-vinyl fluorosilicone oil is 1.2%-1.5% and the active hydrogen mass fraction of the end-hydrogen silicone oil is 0.4%-0.6%, the end-hydrogen silicone oil can fully cross-link and cure with the end-vinyl fluorosilicone oil to form a fluorosilicone rubber layer with a certain strength and hardness, which can not only effectively block the penetration of organic solvents into the pipe body, which is beneficial to improve the organic solvent resistance of PE pipes, but also protect the pipe body, prevent PE pipes from being affected by external factors and causing corrosion, aging, rupture and other problems, which is beneficial to increase the service life of PE pipes. Secondly, when the viscosity of the end-vinyl fluorosilicone oil is 300-500mm 2 / s range, the fluorine-containing silicone coating can have good viscosity and flow properties, can adhere to the inner and outer surfaces of the pipe body, and can fully self-level before completely curing to form a flat protective coating.
[0012] Optionally, the polyimide chopped fibers are subjected to silane modification treatment before mixing, and the silane modification treatment comprises the following steps: The KH550 silane coupling agent and the KH570 silane coupling agent are mixed in a ratio of 1:(0.4-0.6), and added into anhydrous ethanol to prepare a silane-ethanol solution with a concentration of 4%, and then polyimide short fibers are added, heated and stirred, filtered, and the filter residue is soaked and cleaned with deionized water for multiple times, and dried to obtain polyimide short fibers modified with silane.
[0013] By adopting the above technical scheme, the polyimide chopped fibers are modified by mixing KH550 silane coupling agent and KH570 silane coupling agent in proportion, which is beneficial to further improve the compatibility and bonding strength of the polyimide chopped fibers with high-density polyethylene. The use of a compatibilizer can further enable the polyimide chopped fibers to be fully dispersed in the high-density polyethylene, and enable the polyimide chopped fibers to fully exert their reinforcement and anti-seepage effects.
[0014] Optionally, the compatibilizer is maleic anhydride grafted polyethylene.
[0015] By adopting the above technical scheme, maleic anhydride grafted polyethylene can effectively improve the compatibility of polytetrafluoroethylene and polyimide short fibers with high-density polyethylene, so that polytetrafluoroethylene and polyimide short fibers can be fully and evenly mixed in high-density polyethylene, which is beneficial to improving the organic solvent resistance and mechanical strength of PE pipes.
[0016] Optionally, the masterbatch is a masterbatch with high-density polyethylene as a carrier and inorganic pigment as a dye.
[0017] By adopting the above technical solution, since most inorganic pigments are composed of inorganic substances or metal oxides, they are not easy to react chemically with organic solvents, which is beneficial to reduce the influence of organic solvents on the main color of the pipe. Therefore, even if the PE pipe is in contact with organic solvents for a long time, it can still maintain a relatively bright color.
[0018] Optionally, the reinforcing filler is selected from any one or more of nano silicon dioxide or activated calcium carbonate.
[0019] By adopting the above technical solution, both nano-silicon dioxide and activated calcium carbonate can play a certain role in reinforcing and toughening the pipe body, which is beneficial to improving the hydrostatic strength and other mechanical properties of the PE pipe.
[0020] Optionally, the reinforcing filler is a mixture of the nano-silicon dioxide and the activated carbonic acid, and the mixing weight ratio of the nano-silicon dioxide to the activated calcium carbonate is 1:(3-9).
[0021] By adopting the above technical solution, when the reinforcing filler in the pipe body is a mixture of nano-silicon dioxide and activated calcium carbonate in a weight ratio of 1: (3-9), the PE pipe not only has good organic solvent resistance and mechanical strength, but also its preparation cost can be further controlled and reduced.
[0022] Optionally, the antioxidant is a compound of antioxidant 1010 and antioxidant 168, and the weight ratio of the antioxidant 1010 to the antioxidant 168 is 1:(2-3).
[0023] By adopting the above technical solution, when the antioxidant in the pipe body is a mixture of antioxidant 1010 and antioxidant 168 in a weight ratio of 1:(2-3), a certain synergistic effect can be produced between antioxidant 1010 and antioxidant 168, which is beneficial to improving the antioxidant properties of the pipe body, thereby improving the aging resistance of the PE pipe.
[0024] In the second aspect, the present application provides a method for preparing an organic solvent-resistant PE pipe, which adopts the following technical solution: A method for preparing an organic solvent-resistant PE pipe, comprising the following steps: S1. First, heat and dry high-density polyethylene, polytetrafluoroethylene, polyimide short fibers, a compatibilizer, a reinforcing filler and an antioxidant respectively, and then add the high-density polyethylene to an extruder. After the high-density polyethylene is fully melted in the extruder, polytetrafluoroethylene, polyimide short fibers, a compatibilizer, a reinforcing filler and an antioxidant are added in sequence, and the raw materials are fully mixed through the extruder screw. Finally, the raw materials are melt-extruded and vacuum-cooled and shaped through a corresponding pipe mold to obtain a pipe body. S2. Immerse the pipe body obtained in step S1 in the fluorine-containing silicone coating, so that the fluorine-containing silicone coating is evenly coated on the inner and outer sides of the pipe body. After taking out the pipe body, rotate the pipe body around the central axis and keep rotating at 82-86° C. for 3-5 minutes until a smooth protective coating is formed on the surface, thereby obtaining a PE pipe resistant to organic solvents.
[0025] By adopting the above technical solution, each raw material additive is first added step by step, which is conducive to fully mixing each raw material additive and obtaining a pipe body with uniform performance. Then, the fluorine-containing silicone coating is fully and evenly coated on the surface of the pipe body through immersion, rotation and other operations, and the fluorine-containing silicone coating is kept rotating while curing, so that the fluorine-containing silicone coating can be fully leveled on the inner and outer surfaces of the pipe body and form a flat protective layer, which is conducive to fully covering the protective coating and playing a protective role on the pipe body, and is conducive to improving the organic solvent resistance of PE pipes. Secondly, the production process is simple, the required equipment investment is small, and the cost is low, which is conducive to subsequent mass production.
[0026] In summary, the technical solution of this application includes at least one of the following beneficial effects: 1. By adding polytetrafluoroethylene and polyimide chopped fibers, and then combining them with a protective coating formed by curing fluorinated silicone coating, the organic solvent tolerance and low swelling properties of PE pipes can be effectively improved.
[0027] 2. A fluorine-containing silicone coating is prepared by mixing vinyl-terminated fluorosilicone oil with a vinyl content of 1.2%-1.5%, hydrogen-terminated silicone oil with an active hydrogen content of 0.4%-0.6%, chloroplatinic acid and titanium dioxide. The protective coating formed on the inner and outer surfaces of the pipe body can not only block organic solvents from penetrating into the pipe body and improve the organic solvent resistance of the PE pipe, but also the protective coating can protect the pipe body as a whole, thereby improving the service life and appearance retention of the PE pipe. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a cross-sectional view of an organic solvent-resistant PE pipe in Example 1 of the present application.
[0029] Description of reference numerals: 1. Pipe body; 2. Protective coating. DETAILED DESCRIPTION
[0030] The present application is further described in detail below in conjunction with the accompanying drawings, preparation examples, embodiments and comparative examples.
[0031] The high-density polyethylene was purchased from HDPE 100 of Sinopec, with a specific grade of YGH-041T.
[0032] The polyimide chopped fibers are purchased from Suplon fibers of Aoshen New Materials and are made by cutting.
[0033] The maleic anhydride grafted polyethylene was purchased from Coase Chemicals, and the specific brand is W1H.
[0034] The activated calcium carbonate was purchased from Huibin Calcium Industry, and the specific brand is CCR-6525.
[0035] The vinyl-terminated fluorosilicone oil was purchased from Taipuda New Materials, and the specific brand is TPD-FS8019.
[0036] The end-hydrogenated silicone oil was purchased from Zhejiang Chuangji, with the specific brand name being CJ-1200.
[0037] The titanium dioxide was purchased from Pangang Group, and the specific grade was R-248 rutile titanium dioxide.
[0038] Preparation Example [Preparation Example 1-1] A fluorine-containing organosilicon coating comprises the following raw materials: 30 kg of vinyl-terminated fluorosilicone oil, 1.5 kg of hydrogen-terminated silicone oil, 0.12 kg of chloroplatinic acid and 0.3 kg of titanium dioxide.
[0039] In this preparation example, the vinyl-terminated fluorosilicone oil is specifically customized to have a vinyl mass fraction of 1.2% and a viscosity of 500 mm at 25°C. 2 / s, the active hydrogen mass fraction of the specially customized end hydrogen-containing silicone oil is 4%.
[0040] A method for preparing a fluorine-containing organosilicon coating comprises the following steps: Firstly, vinyl-terminated fluorosilicone oil, hydrogen-terminated silicone oil and titanium dioxide are fully stirred, mixed and stored. When used, chloroplatinic acid is added and fully mixed to obtain a fluorine-containing organic silicon coating.
[0041] [Preparation Example 1-2] A fluorine-containing organosilicon coating comprises the following raw materials: 35 kg of vinyl-terminated fluorosilicone oil, 1 kg of hydrogen-terminated silicone oil, 0.15 kg of chloroplatinic acid and 0.45 kg of titanium dioxide.
[0042] In this preparation example, the vinyl-terminated fluorosilicone oil is specifically customized to have a vinyl mass fraction of 1.5% and a viscosity of 300 mm at 25°C. 2 / s, the active hydrogen mass fraction of the specially customized end hydrogen-containing silicone oil is 6%.
[0043] A method for preparing a fluorine-containing organosilicon coating comprises the following steps: Firstly, vinyl-terminated fluorosilicone oil, hydrogen-terminated silicone oil and titanium dioxide are fully stirred, mixed and stored. When used, chloroplatinic acid is added and fully mixed to obtain a fluorine-containing organic silicon coating.
[0044] [Preparation Example 2-1] A silane-modified polyimide chopped fiber comprises the following steps: 500 ml of KH550 silane coupling agent and 200 ml of KH570 silane coupling agent were mixed and added to anhydrous ethanol to prepare a silane-ethanol solution with a concentration of 4%, and then polyimide short fibers were added. The solution was heated to 50° C. and stirred for 30 minutes. The filter residue was filtered and rinsed with deionized water for multiple times, and dried to obtain polyimide short fibers modified with silane.
[0045] [Preparation Example 2-2] A silane-modified polyimide chopped fiber comprises the following steps: 500 ml of KH550 silane coupling agent and 300 ml of KH570 silane coupling agent were mixed and added to anhydrous ethanol to prepare a silane-ethanol solution with a concentration of 4%, and then polyimide short fibers were added. The solution was heated to 50° C. and stirred for 30 minutes. The filter residue was filtered and rinsed with deionized water for multiple times, and dried to obtain polyimide short fibers modified with silane. Example
[0046] [Example 1] A PE pipe resistant to organic solvents, refer to Figure 1 , including a pipe body and a protective coating disposed on the inner and outer surfaces of the pipe body. The protective coating is formed by coating and curing a fluorine-containing silicone coating prepared in [Preparation Example 1] on the surface of the pipe body.
[0047] In this embodiment, the pipe body includes the following materials: 100kg high-density polyethylene, 4kg polytetrafluoroethylene, 4kg polyimide chopped fibers, 2kg compatibilizer, 5kg masterbatch, 5g reinforcing filler and 1.8kg antioxidant.
[0048] Among them, the average length of the polyimide chopped fibers is 6 mm; the compatibilizer is maleic anhydride grafted polyethylene; the masterbatch is a masterbatch with PE as a carrier and an inorganic pigment as a dye, and the specific inorganic pigment is carbon black; the reinforcing filler is activated calcium carbonate; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a weight ratio of 1:2, that is, the added amount of antioxidant 1010 is 0.6 kg, and the added amount of antioxidant 168 is 1.2 kg.
[0049] A method for preparing an organic solvent-resistant PE pipe comprises the following steps: S1. First, high-density polyethylene, polytetrafluoroethylene, polyimide short fibers, a compatibilizer, a reinforcing filler and an antioxidant are placed in circulating hot air at 70°C for low-temperature drying, and then the high-density polyethylene is added to the extruder. After the high-density polyethylene is fully melted, polytetrafluoroethylene, polyimide short fibers, a compatibilizer, a reinforcing filler and an antioxidant are added in sequence. The raw materials are fully mixed through the extruder screw, and finally melt-extruded and vacuum-cooled and shaped through the corresponding pipe mold to obtain a pipe body with a thickness of 5 mm. S2. Immerse the pipe body obtained in step S1 in the fluorine-containing silicone coating, so that the fluorine-containing silicone coating is evenly coated on the inner and outer sides of the pipe body, take out the pipe body and rotate it around the central axis so that the fluorine-containing silicone coating can be evenly leveled, then keep rotating and cure at 86° C. for 3 minutes until a flat protective coating is formed on the surface, thereby obtaining a PE pipe resistant to organic solvents.
[0050] [Example 2] A PE pipe resistant to organic solvents, which differs from [Example 1] in that the raw material formulas of the pipe body and the protective coating are different.
[0051] In this embodiment, the protective coating is formed by coating a fluorine-containing silicone coating prepared in [Preparation Example 2] and curing it on the surface of the pipe body.
[0052] In this embodiment, the pipe body includes the following materials: 100kg high-density polyethylene, 8kg polytetrafluoroethylene, 2kg polyimide chopped fibers, 3kg compatibilizer, 3kg masterbatch, 4kg reinforcing filler and 1.5kg antioxidant.
[0053] Among them, the polyimide chopped fibers are silane-modified polyimide chopped fibers obtained in [Preparation Example 2-1], and the average length is 10 mm; the compatibilizer is maleic anhydride grafted polyethylene; the masterbatch is a masterbatch with PE as a carrier and an inorganic pigment as a dye, and the specific inorganic pigment is carbon black; the reinforcing filler is nano-silicon dioxide; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a weight ratio of 1:3, that is, the addition amount of antioxidant 1010 is 0.375 kg, and the addition amount of antioxidant 168 is 1.125 kg.
[0054] A method for preparing an organic solvent-resistant PE pipe, which differs from [Example 1] in that the curing temperature and curing time of the protective coating are different.
[0055] In this embodiment, the pipe body coated with the fluorine-containing silicone coating is kept rotating and cured at 82° C. for 5 minutes until a smooth protective coating is formed on the surface, thereby obtaining a PE pipe resistant to organic solvents.
[0056] [Example 3] A PE pipe resistant to organic solvents, which differs from [Example 1] in that the polyimide chopped fibers are different.
[0057] In this embodiment, the polyimide chopped fibers are silane-modified polyimide chopped fibers obtained in [Preparation Example 2-1], and the average length is 10 mm.
[0058] [Example 4] A PE pipe resistant to organic solvents, which differs from [Example 3] in that the reinforcing filler is different.
[0059] In this embodiment, the reinforcing filler is replaced by nano-silicon dioxide in equal amounts.
[0060] [Example 5] A PE pipe resistant to organic solvents, which differs from [Example 3] in that the reinforcing filler is different.
[0061] In this embodiment, the reinforcing filler is replaced by an equal amount of a composite mixture of nano-silicon dioxide and activated calcium carbonate, and the mixing weight ratio of nano-silicon dioxide and activated calcium carbonate is 1:9, that is, the addition amount of nano-silicon dioxide is 0.5 kg, and the addition amount of activated calcium carbonate is 4.5 kg.
[0062] [Example 6] A PE pipe resistant to organic solvents, which differs from [Example 3] in that the reinforcing filler is different.
[0063] In this embodiment, the reinforcing filler is replaced by an equal amount of a composite mixture of nano-silicon dioxide and activated calcium carbonate, and the mixing weight ratio of nano-silicon dioxide and activated calcium carbonate is 1:3, that is, the added amount of nano-silicon dioxide is 1 kg, and the added amount of activated calcium carbonate is 3 kg.
[0064] Comparative Example [Example 1] A PE pipe, which differs from [Example 1] in that polytetrafluoroethylene and polyimide chopped fibers are not added, and no protective coating is provided.
[0065] [Comparative Example 2] A PE pipe, which is different from [Example 1] in that the inner and outer surfaces of the pipe body are not provided with a protective coating.
[0066] [Comparative Example 3] A PE pipe, which differs from [Example 1] in that polyimide chopped fibers are not added.
[0067] Performance test data 1. Hydrostatic strength test: According to GB / T 6111-2018 Determination of internal pressure resistance of thermoplastic pipe systems for fluid transportation, the test is conducted, and the examples and comparative examples are recorded for whether rupture, leakage, etc. occur within the specified test pressure and test time. The test medium is water, the test temperature is 20°C, the test pressure is 15MPa, and the specified test time is 100h. If the pipe is damaged or leaks within the specified test time, the test is stopped, the test pressure is reduced by 0.5MPa, and the test is repeated until the tested pipe does not rupture or leak within the specified time, and the maximum test pressure that the pipe can withstand is recorded at this time.
[0068] 2. Organic solvent resistance test: A section was cut from each embodiment and comparative example, and after edge sealing, it was completely immersed in ethyl acetate, heated to 60°C in a constant temperature water bath and kept immersed for 72 hours, and the appearance change of the pipe was observed after it was taken out. Then, the hydrostatic strength test was performed again, and the hydrostatic strength test data of each embodiment and comparative example before and after being immersed in organic solvents were recorded and compared.
[0069] Table 1 Performance test data of PE pipe Combining Example 1 with Comparative Examples 1-3 and the data in Table 1, it can be seen that by adding polytetrafluoroethylene and polyimide chopped fibers to the main body of the pipe, and coating a layer of fluorine-containing silicone coating on the surface of the main body of the pipe and curing it to form a protective coating, not only can the organic solvent resistance of the PE pipe be effectively improved, the swelling of the PE pipe after long-term contact with the organic solvent can be reduced or inhibited, but also the hydrostatic strength of the PE pipe can be further improved, so that the PE pipe can withstand higher internal hydraulic pressure without rupture or leakage. This may be because both polytetrafluoroethylene and polyimide chopped fibers have extremely high chemical stability. By adding a compatibilizer to the PE pipe, the pipe's own tolerance to organic solvents and low swelling can be improved. At the same time, the polyimide chopped fibers can also be used as reinforcing fibers to further reinforce the PE pipe, which can not only improve the rigidity and impact strength of the PE pipe, but also reduce the creep of the PE pipe under long-term load, improve the anti-seepage effect of the main body of the pipe, and thus improve the hydrostatic strength of the PE pipe. Secondly, the protective coating formed by the fluorine-containing silicone coating on the inner and outer surfaces of the pipe body also has excellent chemical stability. It can not only block the penetration of organic solvents into the pipe body to a certain extent to reduce swelling, but also reduce the long-term adhesion or corrosion of organic solvents on the surface of PE pipes, which is beneficial to further improve the organic solvent resistance of PE pipes.
[0070] Combining Example 1 with Example 3 and the data in Table 1, it can be seen that after the polyimide chopped fibers are modified with KH550 silane coupling agent and KH570 silane coupling agent, the hydrostatic strength retained by the PE pipe after long-term hot dipping in organic solvents is slightly improved. This may be because after the modification with the silane coupling agent, the compatibility and bonding strength of the polyimide chopped fibers with high-density polyethylene are further improved, and the use of a compatibilizer is conducive to fully dispersing the polyimide chopped fibers in high-density polyethylene and giving full play to the reinforcement and anti-seepage effects.
[0071] Combined with Examples 3-6 and the data in Table 1, it can be seen that when the reinforcing filler in the pipe body is selected from nano-silicon dioxide and activated calcium carbonate and mixed in a weight ratio of 1: (3-9), the PE pipe still has good hydrostatic strength after long-term hot immersion in organic solvents, and as the proportion of nano-silicon dioxide increases, the hydrostatic strength retained by the PE pipe after long-term hot immersion in organic solvents is higher. This may be because both nano-silicon dioxide and activated calcium carbonate can improve the rigidity and mechanical strength of the pipe body, but because nano-silicon dioxide is more stable and not easy to react with other chemical substances, nano-silicon dioxide can also simultaneously improve the resistance of PE pipes to organic solvents or other acidic and alkaline substances, and is not easy to be corroded. And because the cost of activated calcium carbonate is lower, when nano-silicon dioxide and activated calcium carbonate are mixed in a weight ratio of 1: (3-9), the PE pipe not only has good resistance to organic solvents, but also the preparation cost can be further controlled and reduced.
[0072] This specific implementation manner is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the specific implementation manner as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. An organic solvent-resistant PE pipe, characterized in that: The invention comprises a pipe body and a protective coating disposed on the inner and outer surfaces of the pipe body, wherein the protective coating is formed by coating and curing a fluorine-containing silicone coating on the surface of the pipe body, and the pipe body is made of the following raw materials in parts by weight: High-density polyethylene: 100 parts; Polytetrafluoroethylene: 4-8 parts; Polyimide chopped fibers: 2-4 parts; Compatibilizer: 2-3 parts; Masterbatch: 3-5 parts; Reinforcing filler: 4-5 parts; Antioxidants: 1.5-1.8 parts; Wherein, the length of the polyimide chopped fibers ranges from 6 to 10 mm.
2. The organic solvent-resistant PE pipe according to claim 1, characterized in that: The fluorine-containing silicone coating comprises the following raw materials in parts by weight: Vinyl-terminated fluorosilicone oil: 30-35 parts; End-hydrogenated silicone oil: 1-1.5 parts; Chloroplatinic acid: 0.12-0.15 parts; Rutile titanium dioxide: 0.3-0.45 parts.
3. The organic solvent-resistant PE pipe according to claim 2, characterized in that: in, The vinyl mass fraction of the vinyl-terminated fluorosilicone oil is 1.2%-1.5%, and the viscosity of the vinyl-terminated fluorosilicone oil is 300-500mm 2 / s, the mass fraction of active hydrogen in the terminal hydrogen-containing silicone oil is 0.4%-0.6%.
4. The organic solvent-resistant PE pipe according to claim 1, characterized in that: The polyimide chopped fibers are subjected to silane modification treatment, and the silane modification treatment comprises the following steps: The KH550 silane coupling agent and the KH570 silane coupling agent are mixed in a ratio of 1: (0.4-0.6), and added into anhydrous ethanol to prepare a silane-ethanol solution with a concentration of 4%, and then the polyimide short fibers are added, heated and stirred, filtered, and the filter residue is soaked and cleaned with deionized water for multiple times, and dried to obtain the polyimide short fibers modified with silane.
5. The organic solvent-resistant PE pipe according to claim 1, characterized in that: The compatibilizer is maleic anhydride grafted polyethylene.
6. The organic solvent-resistant PE pipe according to claim 1, characterized in that: The color masterbatch is selected from a color masterbatch using high-density polyethylene as a carrier and inorganic pigments as dyes.
7. The organic solvent-resistant PE pipe according to claim 1, characterized in that: The reinforcing filler is selected from any one or more of nano silicon dioxide or active calcium carbonate.
8. The organic solvent-resistant PE pipe according to claim 7, characterized in that: The reinforcing filler is a mixture of the nano silicon dioxide and the active carbonic acid, and the mixing weight ratio of the nano silicon dioxide to the active calcium carbonate is 1: (3-9).
9. The organic solvent-resistant PE pipe according to claim 1, characterized in that: The antioxidant is a compound of antioxidant 1010 and antioxidant 168, and the weight ratio of the antioxidant 1010 to the antioxidant 168 is 1:(2-3).
10. The method for preparing an organic solvent-resistant PE pipe according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. First, heat and dry high-density polyethylene, polytetrafluoroethylene, polyimide short fibers, a compatibilizer, a reinforcing filler and an antioxidant respectively, and then add the high-density polyethylene to an extruder. After the high-density polyethylene is fully melted in the extruder, polytetrafluoroethylene, polyimide short fibers, a compatibilizer, a reinforcing filler and an antioxidant are added in sequence, and the raw materials are fully mixed through the extruder screw. Finally, the raw materials are melt-extruded and vacuum-cooled and shaped through a corresponding pipe mold to obtain a pipe body. S2. Immerse the pipe body obtained in step S1 in the fluorine-containing silicone coating, so that the fluorine-containing silicone coating is evenly coated on the inner and outer sides of the pipe body. After taking out the pipe body, rotate the pipe body around the central axis and keep rotating at 82-86° C. for 3-5 minutes until a smooth protective coating is formed on the surface, thereby obtaining a PE pipe resistant to organic solvents.