Halogen-free resin composition, electric wire and cable
By adding metal hydroxide and carbon black to the halogen-free resin composition, a resin composition with high flame retardancy, oil resistance and low temperature properties is solved, and the problem of insufficient flame retardancy of cables in the prior art is suitable for Highly demanding wire and cable materials such as railway vehicles.
Patent Information
- Application Number
- CN202410434973.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2024-04-11
- Publication Date
- 2024-11-15
AI Technical Summary
The existing halogen-free flame retardant resin compositions are insufficient when they are suitable for cables of various sizes and structures, and it is difficult to meet the high requirements of flame retardant, oil resistance and low temperature properties such as railway vehicles.
A halogen-free resin composition containing 60 to 70% by mass of crystalline polyolefin and 30 to 40% by mass of maleic anhydride modified polyolefin was used, and 180 to 220 parts by mass of metal hydroxide and 1 to 10 parts by mass of carbon black form a resin composition with high flame retardancy, oil resistance and low temperature properties, and is used for insulating layers and sheathing materials of wires and cables.
The high flame retardancy, oil resistance and low temperature properties of halogen-free resin composition in wires and cables are achieved, and is suitable for high-demand applications such as railway vehicles, improving the safety and reliability of cables.
Smart Images

Figure CN118956045A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a halogen-free resin composition and an electric wire and a cable using the same. Background Art
[0002] Electric wires and cables used in railway vehicles and the like are required to have properties such as flame retardancy, oil resistance, fuel resistance, and low-temperature resistance in addition to general tensile strength and elongation.
[0003] In order to give wires and cables high flame retardancy, materials with brominated flame retardants added to polyolefins are used. However, materials containing a large amount of halogens such as bromine will produce a large amount of toxic gases when burned. Therefore, from the perspective of safety during fires and reducing environmental loads, wires and cables using halogen-free materials that do not contain halogens are becoming more and more popular.
[0004] In particular, wires and cables used in railway vehicles have the risk of accidents due to their defects, so in addition to high flame retardancy, oil resistance, fuel resistance, and low temperature resistance are required in EN standards (EN50264, 50306, etc.).
[0005] For example, Patent Document 1 (Japanese Patent Publication No. 2014-24910) discloses a cable having flame retardancy and improved oil resistance, low temperature characteristics, and damage resistance by using a halogen-free flame retardant resin composition, wherein the halogen-free flame retardant resin composition is composed of a base polymer, a metal hydroxide and carbon black added in a ratio of 150 to 220 parts by mass relative to 100 parts by mass of the base polymer, and the base polymer contains 60 to 70% by mass of a linear low-density polyethylene (LLDPE), 10% by mass or more of an ethylene-vinyl acetate copolymer (EVA) having a melt flow rate (MFR) of 100 or more, and 10 to 20% by mass of a maleic acid-modified polyolefin.
[0006] In addition, patent document 2 (Japanese Patent Gazette No. 2020-125459) discloses a cable, which has flame retardancy and improved oil resistance and low temperature characteristics by using a halogen-free flame retardant resin composition, the halogen-free flame retardant resin composition comprising a base polymer, a metal hydroxide and carbon black; the base polymer comprises 60 to 70 parts by mass of a polyolefin, 10 to 35 parts by mass of a maleic anhydride-modified polyolefin, and 5 to 30 parts by mass of an ethylene vinyl acetate copolymer (EVA); the metal hydroxide is added in a proportion of 150 to 250 parts by mass relative to 100 parts by mass of the base polymer; the carbon black is added in a proportion of 1 to 30 parts by mass relative to 100 parts by mass of the base polymer; the melting point of the above-mentioned polyolefin is above 110°C, and the gel fraction after cross-linking is above 85%.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2014-24910
[0010] Patent Document 2: Japanese Patent Application Publication No. 2020-125459 Summary of the invention
[0011] Problems to be solved by the invention
[0012] It is known that the resin compositions described in Patent Documents 1 and 2 do not have sufficient flame retardancy when applied to cables of various sizes and structures, and further improvement of flame retardancy is desired.
[0013] The present invention has been made in view of the above problems, and an object of the present invention is to provide a halogen-free resin composition having excellent flame retardancy, oil resistance and low-temperature resistance, and an insulated wire and cable using the same.
[0014] Other objects and novel features will become apparent from the description of this specification and the accompanying drawings.
[0015] Methods for solving problems
[0016] A halogen-free resin composition according to one embodiment is a halogen-free resin composition comprising a base polymer, a metal hydroxide and carbon black; the base polymer contains 60 to 70% by mass of a crystalline polyolefin and 30 to 40% by mass of a maleic anhydride-modified polyolefin, and as the crystalline polyolefin, the first crystalline polyolefin having a melting point of 110° C. or higher is contained; relative to 100 parts by mass of the base polymer, the halogen-free resin composition contains 180 to 220 parts by mass of the metal hydroxide and 1 part by mass or more and less than 10 parts by mass of the carbon black.
[0017] In an electric wire according to one embodiment, the insulating layer thereof is composed of the above-mentioned halogen-free resin composition. In an electric cable according to one embodiment, the sheath (coating layer) thereof is composed of the above-mentioned halogen-free resin composition.
[0018] Effects of the Invention
[0019] According to one embodiment, a halogen-free resin composition having excellent flame retardancy, oil resistance, and low-temperature resistance, and an electric wire and a cable using the same can be obtained.
[0020] By using the halogen-free resin composition as a coating material for electric wires and cables, flame retardancy, oil resistance and low-temperature resistance can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a cross-sectional view showing a structural example of an electric wire as one embodiment.
[0022] Figure 2 It is a cross-sectional view showing a structural example of a cable as one embodiment.
[0023] Description of Reference Numerals
[0024] 11: Wire, 11a: Conductor, 11b: Inner insulation layer, 11c: Outer insulation layer, 12: Cable, 12b: Separator, 12c: Shielding braid, 12d: Sheath. DETAILED DESCRIPTION
[0025] Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings. It should be noted that in all the figures used to illustrate the embodiments, the same reference numerals are used to mark the components having the same functions, and their repeated descriptions are omitted. In addition, in the following embodiments, the description of the same or identical parts is not repeated in principle except when particularly necessary.
[0026] <Preliminary research matters>
[0027] The resin compositions described in Patent Documents 1 and 2 are prepared by mixing ethylene vinyl acetate copolymer (EVA) and maleic acid-modified polyolefin into a crystalline polyolefin represented by linear low-density polyethylene (LLDPE).
[0028] It is believed that ethylene vinyl acetate copolymer (EVA) is a component required for mixing a large amount of metal hydroxide in order to ensure sufficient flame retardancy, and further, in Patent Document 2, carbon black is used as a flame retardant auxiliary in order to further improve flame retardancy, and its mixing amount can be increased. That is, in the inventions described in these documents, a metal hydroxide is mixed as a flame retardant in a base polymer obtained by adding EVA to a crystalline polyolefin.
[0029] In addition, the resin compositions described in these patent documents may burn depending on the size of the cable, so the inventors studied the morphology of various resin compositions and cables using the same during combustion. Then, in the process of observing the morphology in detail, it was found that the carbonized layer formed during combustion would foam and become brittle due to the deacetylating of the side chain of EVA contained in the resin composition, and thus the flame retardancy might become lower than expected.
[0030] Therefore, the present inventors have studied on a halogen-free resin composition which is suitable for use in electric wires and cables and has improved flame retardancy, and have found a novel halogen-free resin composition described below.
[0031] <Halogen-free resin composition>
[0032] Hereinafter, the halogen-free resin composition according to the present embodiment will be described in detail.
[0033] As described above, the halogen-free resin composition of the present embodiment includes a base polymer, a metal hydroxide and carbon black, the base polymer contains 60 to 70% by mass of a crystalline polyolefin and 30 to 40% by mass of a maleic anhydride-modified polyolefin, as a crystalline polyolefin, contains a first crystalline polyolefin having a melting point of 110° C. or higher, and contains 180 to 220 parts by mass of a metal hydroxide and 1 part by mass or more and less than 10 parts by mass of carbon black relative to 100 parts by mass of the base polymer.
[0034] [Base polymer]
[0035] The base polymer used in the present embodiment contains (1) a crystalline polyolefin and (2) a maleic anhydride-modified polyolefin. Each component will be described below.
[0036] (1) Crystalline polyolefin
[0037] The crystalline polyolefin used here is a polyolefin having crystallinity. In the present embodiment, the crystalline polyolefin includes a crystalline polyolefin having a melting point of 110° C. or higher. In the present specification, the melting point can be determined by differential scanning calorimetry (DSC). By using such a polyolefin having a melting point of 110° C. or higher, oil resistance can be improved.
[0038] As an oil resistance test, there is a method as follows: after immersing the test piece in IRM902 test oil heated to 100°C for 72 hours, the tensile properties are investigated to confirm the extent to which the tensile properties after immersion change relative to the tensile properties before immersion. For example, if the melting point is lower than 110°C, the crystals melt during the oil resistance test, making it difficult to prevent the oil from diffusing into the base polymer, and the rate of change in the tensile properties increases.
[0039] As polyolefins having a melting point of 110°C or higher, there can be mentioned polyethylenes such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), medium-density polyethylene (MDPE), and high-density polyethylene (HDPE), and polypropylene (PP). However, high-density polyethylene (HDPE) has a high degree of crystallinity and a low elongation at break, and polypropylene (PP) is easily disintegrated during crosslinking such as electron beam irradiation. In order to obtain a balance of properties, low-density polyethylene (LDPE) is preferably used, and linear low-density polyethylene (LLDPE) is more preferably used.
[0040] When the base polymer is set to 100 mass%, the addition amount of the crystalline polyolefin is preferably 60 to 70 mass%. When it is less than 60 mass%, the oil resistance may be insufficient; when it is more than 70 mass%, the low-temperature elongation may not be fully obtained. In addition, when a low molecular weight polyethylene is used as the crystalline polyolefin, the entanglement of the molecules disappears and the elongation may decrease. Therefore, it is preferred to use a polyolefin with an MFR (melt flow rate, JIS K 7210, 190°C, 2.16 kg load) of 10 g / 10 min or less.
[0041] In addition, as the crystalline polyolefin, as the polyolefin having a melting point of 110°C or higher, a crystalline polyethylene having a melting point of 110°C or higher (first crystalline polyolefin) is included, and further, a crystalline polyolefin (other than polyethylene) having a melting point of 100°C or higher different from the first crystalline polyolefin (second crystalline polyolefin) can be used simultaneously. Thus, the flexibility of the wire or cable can be improved while maintaining oil resistance.
[0042] Examples of the second crystalline polyolefin include olefin block copolymers (OBC) such as ethylene block copolymers, ethylene ethyl acrylate copolymers (EEA), and ethylene butyl acrylate copolymers.
[0043] The crystalline polyethylene is preferably a polymer having a heat of fusion of 50 J / g or more, and more preferably a polymer having a heat of fusion of 75 J / g or more. If the heat of fusion is 50 J / g or more, oil resistance can be improved. It should be noted that the heat of fusion is a value measured using a differential scanning calorimeter (DSC) in a temperature range of -50°C to 200°C and a heating rate of 10°C / min.
[0044] When a first crystalline polyolefin composed of polyethylene having a melting point of 110° C. or higher and a second crystalline polyolefin having a melting point of 100° C. or higher are used simultaneously, oil resistance and flexibility can be achieved by making the first crystalline polyolefin 30% by mass or higher and the second crystalline polyolefin 20% by mass or higher. That is, it is preferred that the first crystalline polyolefin be contained in an amount of 30% by mass or higher and 50% by mass or lower in the base polymer, and the second crystalline polyolefin be contained in an amount of 20% by mass or higher and 40% by mass or lower in the base polymer.
[0045] (2) Maleic anhydride modified polyolefin
[0046] The maleic anhydride-modified polyolefin used herein is a compound obtained by modifying a polyolefin with maleic anhydride.
[0047] As the polyolefin used as the modified material (before modification), polyethylene such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), and ultra-low-density polyethylene (VLDPE), ethylene-methyl acrylate copolymer, ethylene-ethyl acrylate copolymer, ethylene-butyl acrylate copolymer, ethylene-1-butene copolymer, ethylene-1-hexene copolymer, ethylene-1-octene copolymer and other ethylene-α-olefins can be cited. Among them, ethylene-1-butene copolymer, ethylene-1-hexene copolymer, and ethylene-1-octene copolymer have less crystallinity and excellent filler acceptance in the resin composition, so they are preferably used as the material of maleic anhydride modified polyolefin.
[0048] The method of modifying the polyolefin before modification with maleic anhydride is not particularly limited, and it can be carried out by a known method, for example, it can also be obtained by a reaction using only heat brought about by heating. In addition, the maleic anhydride in the maleic anhydride-modified polyolefin can be graft copolymerized or block copolymerized.
[0049] The amount of the maleic anhydride-modified polyolefin in 100% by mass of the base polymer is set to 30 to 40% by mass. When it is less than 30% by mass, the required low-temperature properties and flame retardancy may not be satisfied, and when it is more than 40% by mass, the interaction of the filler becomes too strong, the viscosity increases, and the processability during extrusion molding may deteriorate.
[0050] [Metal hydroxide]
[0051] In this embodiment, a metal hydroxide is added to the base polymer as a flame retardant. Examples of the metal hydroxide used here include aluminum hydroxide, magnesium hydroxide, and calcium hydroxide.
[0052] Among them, aluminum hydroxide and magnesium hydroxide are preferably used. The heat absorption when calcium hydroxide decomposes is about 1000 J / g, while the heat absorption of aluminum hydroxide and magnesium hydroxide is 1500-1600 J / g, which is high. Therefore, the flame retardancy is improved by adding aluminum hydroxide and magnesium hydroxide.
[0053] Furthermore, magnesium hydroxide is preferably selected and used. Since magnesium hydroxide has a higher decomposition temperature than aluminum hydroxide, for example, the temperature during molding of the resin composition can be increased, thereby improving molding processability.
[0054] In order to improve dispersibility and the like, the metal hydroxide may be surface-treated with a silane coupling agent, a titanate coupling agent, a fatty acid such as stearic acid, or the like.
[0055] The BET specific surface area of the metal hydroxide is preferably 5.0 or more. When the BET specific surface area is 5.0 or more, the interaction between the polymer and the metal hydroxide becomes stronger, and the tensile strength is improved. It should be noted that the BET specific surface area can be calculated according to the "carrier gas method" of JIS Z 8830:2013 using nitrogen as the adsorbent.
[0056] The metal hydroxide is added in an amount of 180 to 220 parts by mass relative to 100 parts by mass of the base polymer. If the amount is less than 180 parts by mass, sufficient flame retardancy cannot be obtained, and if the amount is more than 220 parts by mass, extrusion moldability is reduced.
[0057] [Carbon black]
[0058] The carbon black used here functions as a colorant. As the carbon black to be added, the type is not particularly limited and known carbon black can be used, but in consideration of elongation at break, etc., FT and MT grade carbon are preferably used.
[0059] The amount of the carbon black is preferably 1 part by mass or more and less than 10 parts by mass, more preferably 1 to 5 parts by mass, relative to 100 parts by mass of the base polymer. In this embodiment, for example, since carbon black is not added as a flame retardant auxiliary as in Patent Document 2, the amount of the carbon black can be the same as that of a colorant known in the past, and sufficient flame retardancy can be ensured even without adding ethylene vinyl acetate copolymer.
[0060] [Other additives]
[0061] Flame retardants, crosslinking agents, crosslinking aids, ultraviolet absorbers, light stabilizers, softeners, lubricants, colorants, reinforcing agents, surfactants, inorganic fillers, antioxidants, plasticizers, metal chelating agents, foaming agents, compatibilizers, processing aids, stabilizers, etc. can be added to the base polymer.
[0062] As flame retardant aids, known flame retardant aids can be used. It should be noted that there are phosphorus flame retardant aids such as red phosphorus, and triazine flame retardant aids such as melamine cyanurate, but they may produce phosphine gas and cyanide gas, so care should be taken when operating. Any flame retardant aid other than these can be used, for example, clay, silicon dioxide, zinc stannate, zinc borate, calcium borate, dolomite hydroxide, silicone, etc. can be used.
[0063] The above-mentioned resin composition has crosslinking properties and is crosslinked to form a crosslinked product. The crosslinking treatment includes chemical crosslinking using organic peroxides, sulfur compounds or silanes, irradiation crosslinking using electron beams or radiation, chemical crosslinking using other chemical reactions, and any crosslinking method can be applied. Among them, irradiation crosslinking using electron beams is more versatile than other irradiation crosslinking, and there is no risk of scorching during extrusion molding like chemical crosslinking, so it is preferably used as the crosslinking treatment of this embodiment.
[0064] <Wires>
[0065] Next, use Figure 1 An electric wire as one embodiment will be described. Figure 1 It is a cross-sectional view showing a structural example of the electric wire according to the present embodiment.
[0066] like Figure 1 As shown, the electric wire 11 of this embodiment includes a conductor 11a, an insulating inner layer 11b formed on the outer periphery of the conductor 11a, and an insulating outer layer 11c formed on the outer periphery of the insulating inner layer 11b. In this way, the insulating layer covering the conductor 11a may be a double-layer structure of the insulating inner layer 11b and the insulating outer layer 11c.
[0067] As the conductor 11a, for example, a stranded wire formed by twisting a plurality of wires (metal wires) can be used. As the wire, for example, in addition to copper wire and copper alloy wire, aluminum wire, gold wire, silver wire, etc., or wire with a metal coating of tin, nickel, etc. applied to the periphery can also be used.
[0068] As the insulating inner layer 11b, for example, polyethylene, polybutylene terephthalate, etc. can be used. In addition, in the inner layer material, additives such as antioxidants, silane coupling agents including silicone rubber, flame retardants, flame retardant aids, crosslinking agents, crosslinking aids, crosslinking accelerators, hydrolysis inhibitors (such as polycarbodiimide compounds), lubricants (such as fatty acid metal salts, amide lubricants), softeners, plasticizers, inorganic fillers, carbon black, compatibilizers, stabilizers, metal chelating agents, ultraviolet absorbers, light stabilizers, and colorants can be added as needed. In addition, as the insulating inner layer 11b, a composition crosslinked by silane water crosslinking or electron beam irradiation can be used.
[0069] As the insulating outer layer 11c, the above-mentioned halogen-free resin composition can be used.
[0070] In addition, other resin compositions with halogen-free flame retardants can also be used as the insulating outer layer 11c. Among the halogen-free flame retardants, it is preferred not to add phosphorus-based flame retardants such as red phosphorus and triazine-based flame retardants such as melamine cyanurate. The polymer suitable for the insulating outer layer 11c is not particularly limited as long as it is halogen-free. For example, polyolefins such as high-density polyethylene (HDPE), medium-density polyethylene (MDPE), low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), ultra-low-density polyethylene (VLDPE), and ethylene-acrylate copolymers can be listed. Rubber materials can also be used, and ethylene-propylene copolymer rubber, ethylene-propylene-diene terpolymer rubber, acrylic rubber, ethylene-acrylate copolymer rubber, ethylene-octene copolymer rubber, ethylene-vinyl acetate copolymer rubber, ethylene-1-butene copolymer rubber, butadiene-styrene copolymer rubber, isobutylene-isoprene copolymer rubber, block copolymer rubber with polystyrene blocks, etc. can be listed. In addition, engineering plastics can also be used, such as polyethylene terephthalate, polybutylene terephthalate, polyphenylene ether, polycarbonate, polyamide, polyphenylene sulfide, polyetheretherketone, polyethylene naphthalate, polybutylene naphthalate, polyethersulfone, etc. These thermoplastic elastomers can also be used. The base polymer can be used alone or in combination of two or more.
[0071] In the insulating outer layer 11c, in the resin composition composed of the above materials, cross-linking agents, cross-linking aids, flame retardants, ultraviolet absorbers, light stabilizers, softeners, lubricants, colorants, reinforcing agents, surfactants, inorganic fillers, plasticizers, metal chelators, foaming agents, compatibilizers, processing aids, stabilizers, etc. can be added as needed.
[0072] From the viewpoint of oil resistance, crosslinking should be performed in advance. The crosslinking treatment includes chemical crosslinking using organic peroxides or silane compounds, crosslinking using irradiation with electron beams, radiation, etc., and crosslinking using other chemical reactions. However, any crosslinking method can be applied.
[0073] By forming a double-layer structure in this way, the electrical insulation can be improved by the insulating inner layer 11 b on the conductor 11 a side, and the flame retardancy can be improved by the insulating outer layer 11 c as the outermost layer.
[0074] It should be noted that in Figure 1 In the embodiment, the insulating layer covering the conductor 11a is a double-layer structure of an insulating inner layer 11b and an insulating outer layer 11c, but may be a three-layer or more structure, or may be a single-layer structure. In either case, by using the aforementioned halogen-free resin composition as the outermost layer, the characteristics of the halogen-free insulated wire can be improved.
[0075] The electric wire 11 of the present embodiment is manufactured, for example, as follows. First, a resin composition for forming the insulating inner layer 11b and the insulating outer layer 11c is prepared. In the present embodiment, as a resin composition having this feature, for example, a material including a crystalline polyolefin and a maleic anhydride-modified polyolefin as a base polymer, a metal hydroxide, and carbon black is melt-kneaded to obtain the resin composition of the present embodiment.
[0076] Then, the conductor 11a is prepared. Then, the resin composition is extruded by an extruder so as to cover the conductor 11a to form an insulating inner layer 11b, and then the resin composition of this embodiment is extruded so as to cover the insulating inner layer 11b to form an insulating outer layer 11c. Furthermore, the resin composition is cross-linked as needed to manufacture the electric wire 11.
[0077] <Cable>
[0078] Next, use Figure 2 A cable as one embodiment will be described. Figure 2 It is a cross-sectional view showing a structural example of the cable according to the present embodiment.
[0079] like Figure 2 As shown, the cable 12 of this embodiment has two twisted wires 11 (twisted core, see Figure 1 ), a separator 12b disposed outside the twisted core, a shielding braid 12c disposed in a manner covering the separator, and a sheath (outer coating, coating) 12d covering the shielding braid 12c. By using the aforementioned halogen-free resin composition as the sheath 12d, the characteristics of the halogen-free cable can be improved.
[0080] It should be noted that the wire 11 may be one or more than three. The material of the separator 12b is not particularly limited, and the separator 12b may be disposed outside the shielding braid 12c. In order to exert a shielding effect, the shielding braid 12c is made of a conductor material represented by a metal material.
[0081] Such electric wires and cables can be used for any purpose, and can be used, for example, as insulated electric wires or cables for railway vehicles.
[0082] The cable 12 of the present embodiment is manufactured, for example, as follows. First, two electric wires 11 are manufactured by the above method. Then, the two electric wires 11 are twisted together with an intermediary such as rayon, paper tape, jute, etc., and then, in a manner of covering them, a separator 12b and a shielding braid 12c are formed in this order by a known method. Furthermore, the resin composition of the present embodiment is extruded on the outer periphery of the shielding braid 12c obtained in this way, in the same manner as the manufacturing method of the above-mentioned electric wire, to form a sheath 12d of a predetermined thickness. In this way, the cable 12 of the present embodiment can be manufactured.
[0083] In the above, although the case where the electric wire 11 is used in the cable 12 of the present embodiment is described as an example, the present invention is not limited thereto, and an electric wire using a general-purpose material for the insulating layer may be used.
[0084] Example
[0085] Hereinafter, the halogen-free resin composition, electric wire, and cable according to the present embodiment will be described in further detail with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples.
[0086] <Preparation of halogen-free resin composition>
[0087] In Examples 1 to 11, halogen-free resin compositions were prepared according to the formulations shown in Table 1, and in Comparative Examples 1 to 5, halogen-free resin compositions were prepared according to the formulations shown in Table 2. The units of the blending amounts in Tables 1 and 2 are parts by mass. That is, the blending materials shown in Tables 1 and 2 were kneaded using a pressure kneader, extruded in a strip shape, and cooled to form pellets. The blending ratios of the halogen-free resin compositions of the Examples and Comparative Examples will be described in detail later.
[0088] <Manufacturing of electric wires and cables>
[0089] First, make the wires (see Figure 1 Here, 19 tinned copper conductors with a diameter of 0.18 mm were used as the conductor 11a. Polybutylene terephthalate (manufactured by Mitsubishi Engineering-Plastics Corporation, trade name: NOVADURAN 5026) was used as the insulating inner layer 11b. As the insulating outer layer 11c, a material obtained by kneading 30 parts by mass of polyethylene (manufactured by PRIME POLYMER, trade name: HI-ZEX 5305E), 30 parts by mass of ethylene-ethyl acrylate-maleic anhydride terpolymer (manufactured by ARKEMA, trade name: BONDINE LX 4110), 10 parts by mass of maleic anhydride-modified ethylene-α-olefin (manufactured by Mitsui Chemicals, trade name: TAFMERMA 7020), 30 parts by mass of ethylene-ethyl acrylate copolymer (manufactured by Japan Polyethylene Co., Ltd., trade name: REXPEARLA 1150), and 150 parts by mass of magnesium hydroxide (manufactured by Kyowa Chemical Co., Ltd., trade name: KISUMA 5L) using a 14-inch open roll and granulating with a granulator is used. The conductor 11a was covered with the inner insulating layer 11b and the outer insulating layer 11c by double extrusion using a 40 mm extruder so that the thickness of the inner insulating layer 11b was 0.1 mm and the thickness of the outer insulating layer 11c was 0.16 mm. The obtained electric wire 11 was crosslinked by irradiating electron beams.
[0090] Next, a cable is manufactured using the electric wire 11 (see Figure 2 ) Two obtained electric wires 11 were twisted to form a twisted core, on which a 32 μm polyethylene terephthalate separator 12b was overlapped and wound, and on which a shield braid 12c with a braiding density of 80% was formed using a 0.11 mm tinned copper conductor to form a core.
[0091] The composition shown in Table 1 and Table 2 was extruded on the core to a thickness of 0.7 mm using a 40 mm extruder to form a sheath 12d. The obtained sheath 12d of the cable was irradiated with electron beams at the irradiation amount shown in Table 1 and Table 2 to crosslink the sheath 12d, thereby manufacturing the cable 12. The detailed operation of manufacturing the cable 12 will be described later.
[0092] <Evaluation and judgment>
[0093] The sheath 12d of the cable 12 obtained above was tested and evaluated for its extrusion moldability, tensile strength, elongation, oil-resistant tensile strength residual rate, oil-resistant elongation residual rate, low-temperature elongation, and flame retardancy as follows. The results are summarized in Tables 1 and 2.
[0094] [Extrusion moldability]
[0095] In the extrusion molding of the sheath, if the extrusion molding could be performed without any problem, it was evaluated as ○ (good), and if the extrusion molding could not be performed due to the high viscosity of the halogen-free resin composition, it was evaluated as × (unacceptable).
[0096] [Tensile test]
[0097] The twisted core is pulled out from the obtained cable, and the tubular sheath is punched out using a No. 6 dumbbell to obtain a test piece. The test piece is stretched at a displacement speed of 250 mm / min at room temperature (25°C), and the load until break and the elongated length (Lb) are measured. The tensile strength (unit (MPa)) is calculated from the above load. In addition, the elongation at break is calculated based on the initial length La and the elongated length Lb ((Lb-La) / La)×100[%]). The elongation at break of 200% or more is set as ◎ (excellent), 150% or more and less than 200% is set as ○ (good), and less than 150% is set as × (unacceptable).
[0098] [Low temperature test]
[0099] The twisted core etc. is pulled out from the obtained cable, and the tubular sheath is punched out using a No. 6 dumbbell to obtain a test piece. The test piece is kept at -50°C, stretched at a displacement speed of 25 mm / min in an atmosphere of -50°C, and the elongation (L2) until it breaks is measured. Based on the initial length L1 and the elongation L2, the low-temperature elongation ((L2 / L1)×100[%]) is calculated. A low-temperature elongation of 50% or more is set as ◎ (excellent), 30% or more and less than 50% is set as ○ (good), and less than 30% is set as × (unacceptable).
[0100] [Oil resistance test]
[0101] The twisted core etc. was pulled out from the cable, and the tubular sheath was punched out using a No. 6 dumbbell to obtain a test piece. After the test piece was immersed in the IRM902 test oil heated to 100°C for 72 hours, the test piece was stretched at a displacement speed of 250 mm / min, and the stress and elongation until fracture were measured. The residual rate of oil-resistant tensile strength ((A2 / A1)×100[%]) and the residual rate of oil-resistant elongation at break ((B2 / B1)×100[%]) were calculated from the tensile strength (A1) and elongation at break (B1) of the test piece before immersion in the test oil, and the tensile strength (A2) and elongation at break (B2) of the test piece after immersion in the test oil.
[0102] When the residual rate of oil-resistant tensile strength was within the range of 70 to 130%, it was rated as ○ (good), and when it was outside the range of 70 to 130%, it was rated as × (unacceptable). In particular, when it was within the range of 85 to 115%, it was rated as ◎ (excellent).
[0103] When the oil-resistant elongation at break residual ratio was within the range of 60 to 140%, it was rated as ○ (good), and when it was outside the range of 60 to 140%, it was rated as × (unacceptable). In particular, when it was within the range of 80 to 120%, it was rated as ◎ (excellent).
[0104] [Combustion test (flame retardancy)]
[0105] A cable of 600 mm in length is cut out as a test piece, and the test piece is held vertically. If the test piece is in contact with the flame for 60 seconds and then the flame is removed, the test piece that self-extinguishes is set to ◎ (excellent). For the test piece that does not self-extinguish, the test piece is changed and the same test is continued for 2 more times. Even if it self-extinguishes once in 3 tests, it is set to ○ (good). For the test piece that does not self-extinguish in 3 times, a 60° tilt is applied, and the test piece is held vertically. If the flame is removed after 60 seconds of contact with the flame, the test piece that self-extinguishes is set to △ (acceptable). The test piece that does not self-extinguish in this 60° tilted combustion test is set to × (unacceptable).
[0106] [Comprehensive evaluation]
[0107] As a comprehensive evaluation, in the evaluation of the above-mentioned properties other than extrusion moldability (tensile test (elongation at break), low temperature test (low temperature elongation), oil resistance test (oil resistance tensile strength residual, oil resistance elongation at break residual), combustion test (flame retardancy)), the case where all ◎ was set to ◎ (excellent), the case where ○ was included was set to ○ (good), and the case where × was included was set to × (unacceptable).
[0108] [Table 1]
[0109]
[0110] [Table 2]
[0111]
[0112] (Example 1)
[0113] 60 parts by mass of crystalline polyolefin 1 (LLDPE, manufactured by PRIME POLYMER, trade name: SP 1510, melting point 117°C), 40 parts by mass of modified polyolefin 1 (maleic anhydride modified polyolefin, manufactured by Mitsui Chemicals, trade name: TAFMER MH 7020), 180 parts by mass of metal hydroxide 1 (magnesium hydroxide, manufactured by Kamishima Chemical Co., Ltd., trade name: MAGSEEDS S4), 2 parts by mass of colorant (carbon black, manufactured by Asahi Carbon Co., Ltd., trade name: ASAHI-THERMAL), 2 parts by mass of antioxidant 1 (phenolic antioxidant, manufactured by BASF, trade name: IRGANOX 1010), 2 parts by mass of antioxidant 2 (composite antioxidant, manufactured by ADEKA, trade name: ADKSTAB 1 part by mass of 1,2-dimethyl-2-nitropropane trimethacrylate (TMPT, manufactured by Shin-Nakamura Chemical Co., Ltd.) and 1 part by mass of 1,2-dimethyl-2-nitropropane trimethacrylate (TMPT, manufactured by Shin-Nakamura Chemical Co., Ltd.) were mixed to prepare a halogen-free resin composition. This was used as a material for the sheath to manufacture a cable as described above. In Example 1, electron beam irradiation was performed at 75 kGy.
[0114] According to Table 1, in Example 1, all the properties (except extrusion moldability) were rated ◎, and the comprehensive evaluation was rated ◎.
[0115] (Example 2)
[0116] 60 parts by mass of crystalline polyolefin 1 (LLDPE, manufactured by PRIME POLYMER, trade name: SP 1510, melting point 117°C), 30 parts by mass of modified polyolefin 1 (maleic anhydride modified polyolefin, manufactured by Mitsui Chemicals, trade name: TAFMER MH 7020), 10 parts by mass of modified polyolefin 2 (maleic anhydride modified polyolefin, manufactured by Mitsui Chemicals, trade name: TAFMER MH 5040), 220 parts by mass of metal hydroxide 2 (aluminum hydroxide, manufactured by Huber, trade name: MARTIAN L OL-104C), 2 parts by mass of colorant (carbon black, manufactured by Asahi Carbon, trade name: ASAHI-THERMAL), 2 parts by mass of antioxidant 1 (phenolic antioxidant, manufactured by BASF, trade name: IRGANOX 1010), 2 parts by mass of antioxidant 2 (composite antioxidant, manufactured by ADEKA, trade name: ADKSTAB AO-18) 1 part by mass, lubricant (zinc stearate, manufactured by Sakai Chemical Co., Ltd., trade name: SZ-P) 1 part by mass, crosslinking aid (trimethylolpropane trimethacrylate (TMPT, manufactured by Shin-Nakamura Chemical Co., Ltd.) 4 parts by mass were mixed to obtain a halogen-free resin composition, and a cable using the halogen-free resin composition as a sheath material was manufactured. In Example 2, electron beam irradiation was performed at 125 kGy.
[0117] According to Table 1, in Example 2, all the characteristics were ◎ or ○, and the comprehensive evaluation was ○.
[0118] (Example 3 to Example 6)
[0119] 30 to 40 parts by mass of crystalline polyolefin 1 (LLDPE, manufactured by PRIME POLYMER, trade name: SP 1510, melting point 117°C), 30 to 40 parts by mass of crystalline polyolefin 2 (olefin block copolymer (OBC), manufactured by Dow Chemical, trade name: INFUSE 9100, melting point 120°C), 30 parts by mass of modified polyolefin 1 (maleic anhydride-modified polyolefin, manufactured by Mitsui Chemicals, trade name: TAFMER MH 7020), 30 parts by mass of metal hydroxide 1 (magnesium hydroxide, manufactured by Kamishima Chemical, trade name: MAGSEEDS S4), 180 to 200 parts by mass of colorant (carbon black, manufactured by Asahi Carbon, trade name: ASAHI-THERMAL), 2 parts by mass of antioxidant 1 (phenolic antioxidant, manufactured by BASF, trade name: IRGANOX 1010), 2 parts by mass of antioxidant 2 (composite antioxidant, manufactured by ADEKA, trade name: ADKSTAB AO-18), 1 part by mass of lubricant (zinc stearate, manufactured by Sakai Chemical Co., Ltd., trade name: SZ-P), 1 part by mass of crosslinking aid (trimethylolpropane trimethacrylate (TMPT), manufactured by Shin-Nakamura Chemical Co., Ltd.), were mixed to obtain a halogen-free resin composition, and a cable using the halogen-free resin composition as a sheath material was manufactured. In Examples 3 to 6, the wire was irradiated with 125 kGy.
[0120] According to Table 1, in Examples 3 to 6, all the characteristics were ◎ or ○, and the overall evaluation was ○.
[0121] (Example 7 to Example 10)
[0122] 30 to 40 parts by mass of crystalline polyolefin 1 (LLDPE, manufactured by PRIME POLYMER, trade name: SP 1510, melting point 117°C), 30 to 40 parts by mass of crystalline polyolefin 2 (olefin block copolymer (OBC), manufactured by Dow Chemical, trade name: INFUSE 9100, melting point 120°C), 30 parts by mass of modified polyolefin 2 (maleic anhydride modified polyolefin, manufactured by Mitsui Chemicals, trade name: TAFMER MH 5040), 30 parts by mass of metal hydroxide 1 (magnesium hydroxide, manufactured by Kamishima Industries, trade name: MAGSEEDS S4), 180 to 200 parts by mass of colorant (carbon black, manufactured by Asahi Carbon, trade name: ASAHI-THERMAL), 2 parts by mass of antioxidant 1 (phenolic antioxidant, manufactured by BASF, trade name: IRGANOX 1010), 2 parts by mass of antioxidant 2 (composite antioxidant, manufactured by ADEKA, trade name: ADKSTAB AO-18), 1 part by mass of lubricant (zinc stearate, manufactured by Sakai Chemical Co., Ltd., trade name: SZ-P), 1 part by mass of crosslinking aid (trimethylolpropane trimethacrylate (TMPT), manufactured by Shin-Nakamura Chemical Co., Ltd.), were mixed to obtain a halogen-free resin composition, and a cable using the halogen-free resin composition as a sheath material was manufactured. In Examples 7 to 10, electron beam irradiation was performed at 125 kGy.
[0123] According to Table 1, in Examples 7 to 10, all the characteristics were ◎ or ○, and the comprehensive evaluation was also ○.
[0124] (Example 11)
[0125] 40 parts by mass of crystalline polyolefin 1 (LLDPE, manufactured by PRIME POLYMER, trade name: SP 1510, melting point 117°C), 30 parts by mass of crystalline polyolefin 3 (ethylene-ethyl acrylate copolymer (EEA), manufactured by Nippon Polyethylene Co., Ltd., trade name: A3100, melting point 104°C), 30 parts by mass of modified polyolefin 1 (maleic anhydride-modified polyolefin, manufactured by Mitsui Chemicals, trade name: TAFMER MH 7020), 180 parts by mass of metal hydroxide 1 (magnesium hydroxide, manufactured by Kamishima Chemical Co., Ltd., trade name: MAGSEEDS S4), 2 parts by mass of colorant (carbon black, manufactured by Asahi Carbon Co., Ltd., trade name: ASAHI-THERMAL), 2 parts by mass of antioxidant 1 (phenolic antioxidant, manufactured by BASF, trade name: IRGANOX 1010), 2 parts by mass of antioxidant 2 (composite antioxidant, manufactured by ADEKA, trade name: ADKSTAB AO-18) 1 part by mass, lubricant (zinc stearate, manufactured by Sakai Chemical Co., Ltd., trade name: SZ-P) 1 part by mass, crosslinking aid (trimethylolpropane trimethacrylate (TMPT, manufactured by Shin-Nakamura Chemical Co., Ltd.) 4 parts by mass were mixed to obtain a halogen-free resin composition, and a cable using the halogen-free resin composition as a sheath material was prepared. In Example 11, electron beam irradiation was performed at 100 kGy.
[0126] According to Table 1, in Example 11, all the characteristics were ◎ or ○, and the comprehensive evaluation was also ○.
[0127] (Comparative Example 1)
[0128] 55 parts by mass of crystalline polyolefin 1 (LLDPE, manufactured by PRIME POLYMER, trade name: SP 1510, melting point 117°C), 15 parts by mass of non-crystalline non-crystalline polyolefin (ethylene vinyl acetate copolymer (EVA), manufactured by Dow Mitsui Chemicals, trade name: EV45X), 30 parts by mass of modified polyolefin 3 (maleic anhydride modified polyolefin, manufactured by Mitsui Chemicals, trade name: TAFMER MH 7010), 180 parts by mass of metal hydroxide 1 (magnesium hydroxide, manufactured by Kamishima Chemical Co., Ltd., trade name: MAGSEEDS S4), 2 parts by mass of colorant (carbon black, manufactured by Asahi Carbon Co., Ltd., trade name: ASAHI-THERMAL), 2 parts by mass of antioxidant 1 (phenolic antioxidant, manufactured by BASF, trade name: IRGANOX 1010), 2 parts by mass of antioxidant 2 (composite antioxidant, manufactured by ADEKA, trade name: ADKSTAB AO-18) 1 part by mass, lubricant (zinc stearate, manufactured by Sakai Chemical Co., Ltd., trade name: SZ-P) 1 part by mass, crosslinking aid (trimethylolpropane trimethacrylate (TMPT, manufactured by Shin-Nakamura Chemical Co., Ltd.) 4 parts by mass were mixed to obtain a halogen-free resin composition, and a cable using the halogen-free resin composition as a sheath material was manufactured. In Comparative Example 1, electron beams were irradiated at 75 kGy.
[0129] According to Table 2, in Comparative Example 1, the content of crystalline polyolefin was insufficient, so the oil resistant tensile strength residual ratio did not fall within the range of 70 to 130%, and the low temperature elongation was less than 30%, and the evaluations were respectively ×, so the overall evaluation was ×.
[0130] (Comparative Example 2)
[0131] 50 parts by mass of crystalline polyolefin 1 (LLDPE, manufactured by PRIME POLYMER, trade name: SP 1510, melting point 117°C), 30 parts by mass of crystalline polyolefin 3 (ethylene-ethyl acrylate copolymer (EEA), manufactured by Nippon Polyethylene Co., Ltd., trade name: A3100, melting point 104°C), 20 parts by mass of modified polyolefin 1 (maleic anhydride-modified polyolefin, manufactured by Mitsui Chemicals, trade name: TAFMER MH7020), 180 parts by mass of metal hydroxide 1 (magnesium hydroxide, manufactured by Kamishima Chemical Co., Ltd., trade name: MAGSEEDS S4), 2 parts by mass of colorant (carbon black, manufactured by Asahi Carbon Co., Ltd., trade name: ASAHI-THERMAL), 2 parts by mass of antioxidant 1 (phenolic antioxidant, manufactured by BASF, trade name: IRGANOX 1010), 2 parts by mass of antioxidant 2 (composite antioxidant, manufactured by ADEKA, trade name: ADKSTAB AO-18) 1 part by mass, lubricant (zinc stearate, manufactured by Sakai Chemical Co., Ltd., trade name: SZ-P) 1 part by mass, crosslinking aid (trimethylolpropane trimethacrylate (TMPT, manufactured by Shin-Nakamura Chemical Co., Ltd.) 4 parts by mass were mixed to obtain a halogen-free resin composition, and a cable using the halogen-free resin composition as a sheath material was manufactured. In Comparative Example 2, electron beam irradiation was performed at 75 kGy.
[0132] According to Table 2, in Comparative Example 2, the content of the modified polyolefin was insufficient, so the low-temperature elongation was less than 30%, which was evaluated as ×, and the overall evaluation was ×.
[0133] (Comparative Example 3)
[0134] 50 parts by mass of crystalline polyolefin 1 (LLDPE, manufactured by PRIME POLYMER, trade name: SP 1510, melting point 117°C), 30 parts by mass of modified polyolefin 1 (maleic anhydride modified polyolefin, manufactured by Mitsui Chemicals, trade name: TAFMER MH 7020), 20 parts by mass of modified polyolefin 2 (maleic anhydride modified polyolefin, manufactured by Mitsui Chemicals, trade name: TAFMER MH 7040), 240 parts by mass of metal hydroxide 3 (aluminum hydroxide, manufactured by Huber, trade name: MARTIAN L OL-104C), 2 parts by mass of colorant (carbon black, manufactured by Asahi Carbon, trade name: ASAHI-THERMAL), 2 parts by mass of antioxidant 1 (phenolic antioxidant, manufactured by BASF, trade name: IRGANOX 1010), 2 parts by mass of antioxidant 2 (composite antioxidant, manufactured by ADEKA, trade name: ADKSTAB AO-18) 1 part by mass, lubricant (zinc stearate, manufactured by Sakai Chemical Co., Ltd., trade name: SZ-P) 1 part by mass, crosslinking aid (trimethylolpropane trimethacrylate (TMPT, manufactured by Shin-Nakamura Chemical Co., Ltd.) 4 parts by mass were mixed to obtain a halogen-free resin composition, and a cable using the halogen-free resin composition as a sheath material was manufactured. In Comparative Example 3, electron beam irradiation was performed at 75 kGy.
[0135] According to Table 2, in Comparative Example 3, the amount of metal hydroxide added was large and the amount of modified polyolefin was also large, so the elongation at break was less than 150%, which was evaluated as ×, and the overall evaluation was ×.
[0136] (Comparative Example 4)
[0137] 40 parts by mass of crystalline polyolefin 1 (LLDPE, manufactured by PRIME POLYMER, trade name: SP 1510, melting point 117°C), 50 parts by mass of crystalline polyolefin 3 (ethylene-ethyl acrylate copolymer (EEA), manufactured by Japan Polyethylene Co., Ltd., trade name: A3100, melting point 104°C), 10 parts by mass of modified polyolefin 1 (maleic anhydride-modified polyolefin, manufactured by Mitsui Chemicals, trade name: TAFMER MH 7020), 160 parts by mass of metal hydroxide 2 (aluminum hydroxide, manufactured by Huber, trade name: MARTINANLOL-104ZO), 2 parts by mass of colorant (carbon black, manufactured by Asahi Carbon Co., Ltd., trade name: ASAHI-THERMAL), 2 parts by mass of antioxidant 1 (phenolic antioxidant, manufactured by BASF, trade name: IRGANOX 1010), 2 parts by mass of antioxidant 2 (composite antioxidant, manufactured by ADEKA, trade name: ADKSTAB AO-18) 1 part by mass, lubricant (zinc stearate, manufactured by Sakai Chemical Co., Ltd., trade name: SZ-P) 1 part by mass, crosslinking aid (trimethylolpropane trimethacrylate (TMPT, manufactured by Shin-Nakamura Chemical Co., Ltd.) 4 parts by mass were mixed to obtain a halogen-free resin composition, and a cable using the halogen-free resin composition as a sheath material was prepared. In Comparative Example 4, electron beam irradiation was performed at 125 kGy.
[0138] According to Table 2, in Comparative Example 4, the content of the metal hydroxide was insufficient, so the flame retardancy test was rated as ×, and the overall evaluation was rated as ×.
[0139] (Comparative Example 5)
[0140] 60 parts by mass of crystalline polyolefin 1 (LLDPE, manufactured by PRIME POLYMER, trade name: SP 1510, melting point 117°C), 30 parts by mass of non-crystalline polyolefin (ethylene vinyl acetate copolymer (EVA), manufactured by Dow Mitsui Chemicals, trade name: EV45X), 10 parts by mass of modified polyolefin 1 (maleic anhydride-modified polyolefin, manufactured by Mitsui Chemicals, trade name: TAFMER MH 7020), 180 parts by mass of metal hydroxide 2 (aluminum hydroxide, manufactured by Huber, trade name: MARTIANLOL-104ZO), 2 parts by mass of colorant (carbon black, manufactured by Asahi Carbon, trade name: ASAHI-THERMAL), 2 parts by mass of antioxidant 1 (phenolic antioxidant, manufactured by BASF, trade name: IRGANOX 1010), 2 parts by mass of antioxidant 2 (composite antioxidant, manufactured by ADEKA, trade name: ADKSTAB AO-18) 1 part by mass, lubricant (zinc stearate, manufactured by Sakai Chemical Co., Ltd., trade name: SZ-P) 1 part by mass, crosslinking aid (trimethylolpropane trimethacrylate (TMPT, manufactured by Shin-Nakamura Chemical Co., Ltd.) 4 parts by mass were mixed to obtain a halogen-free resin composition, and a cable using the halogen-free resin composition as a sheath material was prepared. In Comparative Example 5, electron beam irradiation was performed at 75 kGy.
[0141] According to Table 2, in Comparative Example 5, the content of the modified polyolefin was insufficient, so the low-temperature elongation was less than 30%, which was evaluated as ×, and the overall evaluation was ×.
[0142] From the above results, Examples 1 to 11 are excellent halogen-free resin compositions that are good in all evaluations, are halogen-free, maintain oil resistance and low-temperature properties, and have improved flame retardancy, and are suitable for insulating layers of electric wires and sheaths (coatings) of cables.
[0143] Although the present invention has been described through the above-mentioned embodiments and examples, the present invention is not limited to the above-mentioned embodiments and examples, and various modifications can be made without departing from the gist of the invention.
[0144] Industrial availability
[0145] The halogen-free resin composition of the present invention can be used not only for halogen-free and flame-retardant wires and cables, but also for sheets, films, panels, pads, tubes, protective materials, fillers, fibers, resin molded products, resin substrates, stationery, building materials, connectors, bushings, ferrules, terminal seats, terminal internal insulators, etc. that require halogen-free flame retardancy.
Claims
1. A halogen-free resin composition comprising a base polymer, a metal hydroxide and carbon black, The base polymer contains 60 to 70% by mass of a crystalline polyolefin and 30 to 40% by mass of a maleic anhydride-modified polyolefin, wherein the crystalline polyolefin contains a crystalline polyolefin having a melting point of 110° C. or higher. The halogen-free resin composition contains 180 to 220 parts by mass of the metal hydroxide and 1 part by mass or more and less than 10 parts by mass of the carbon black relative to 100 parts by mass of the base polymer. The halogen-free resin composition has cross-linking properties.
2. A halogen-free resin composition comprising a base polymer, a metal hydroxide and carbon black, The base polymer contains 60 to 70% by mass of a crystalline polyolefin and 30 to 40% by mass of a maleic anhydride-modified polyolefin, wherein the crystalline polyolefin contains a crystalline polyolefin having a melting point of 110° C. or higher. The halogen-free resin composition contains 180 to 220 parts by mass of the metal hydroxide and 1 part by mass or more and less than 10 parts by mass of the carbon black relative to 100 parts by mass of the base polymer. The halogen-free resin composition is a cross-linked product of the base polymer subjected to a cross-linking treatment.
3. The halogen-free resin composition according to claim 1 or 2, wherein As the base polymer, no ethylene vinyl acetate copolymer is contained.
4. The halogen-free resin composition according to claim 1 or 2, wherein The crystalline polyolefin includes a first crystalline polyolefin which is polyethylene having a melting point of 110° C. or higher and a second crystalline polyolefin which is polyolefin having a melting point of 100° C. or higher, wherein the second crystalline polyolefin does not include polyethylene. The base polymer contains 30% by mass or more of the first crystalline polyolefin and 20% by mass or more of the second crystalline polyolefin, The halogen-free resin composition contains 180 to 220 parts by mass of the metal hydroxide based on 100 parts by mass of the base polymer.
5. The halogen-free resin composition according to claim 1 or 2, wherein The crystalline polyolefin is a polymer having a heat of fusion of 50 J / g or more.
6. The halogen-free resin composition according to claim 1 or 2, wherein The BET specific surface area of the metal hydroxide is greater than 5.
0.
7. An electric wire comprising a conductor and an insulating layer provided around the conductor, The insulating layer is composed of a halogen-free resin composition, which includes a base polymer, a metal hydroxide and carbon black, wherein the base polymer contains 60 to 70% by mass of a first crystalline polyolefin having a melting point of 110° C. or higher and 30 to 40% by mass of a maleic anhydride-modified polyolefin, and the halogen-free resin composition contains 180 to 220 parts by mass of the metal hydroxide and 1 part by mass or more and less than 10 parts by mass of the carbon black relative to 100 parts by mass of the base polymer.
8. A cable comprising an electric wire and a coating layer provided on the outer side thereof, The coating layer is composed of a halogen-free resin composition, which includes a base polymer, a metal hydroxide and carbon black, wherein the base polymer contains 60 to 70% by mass of a first crystalline polyolefin having a melting point of 110° C. or higher and 30 to 40% by mass of a maleic anhydride-modified polyolefin, and the halogen-free resin composition contains 180 to 220 parts by mass of the metal hydroxide and 1 part by mass or more and less than 10 parts by mass of the carbon black relative to 100 parts by mass of the base polymer.