Polyvinyl chloride cable material and preparation method thereof

The prepared PVC cable material solves the PVC cable material resistance in the prior art by using linear polyvinyl chloride resin with an average polymerization degree of 1400-1600 and halogen-free phosphorus-containing flame retardant and trioctyl trimelite. The problems of flammability and transparency achieve excellent flame retardant performance and high transparency, and are suitable for wire and cable insulation layers.

CN118956069APending Publication Date: 2024-11-15LTK INDS HUIZHOU +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411024172.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing polyvinyl chloride (PVC) cable materials produce a large amount of black smoke when burning at high temperatures. The flame retardant performance is poor in the test of extreme oxygen index and UL-94 flame retardant grades, and the addition of non-flame retardant plasticizers reduces its resistance. Flameability leads to a decrease in flame retardancy.

Method used

Using linear polyvinyl chloride resin with an average polymerization degree of 1400-1600, halogen-free phosphorus-containing flame retardant and trioctyl trimellite as raw materials, PVC cable material is prepared through specific mixing and processing processes to improve its Flame retardant properties and transparency.

Benefits of technology

It realizes comprehensive mechanical properties of PVC cable materials with an extreme oxygen index range of 33%-35%, UL-94 flame retardant grade V-0, low smoke density, high visible light transmittance and excellent, satisfying flame retardant performance and transparency Requirements, while improving its physical structural stability during combustion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004968082640000041
    Figure BDA0004968082640000041
  • Figure BDA0004968082640000042
    Figure BDA0004968082640000042
  • Figure BDA0004968082640000081
    Figure BDA0004968082640000081
Patent Text Reader

Abstract

The invention relates to a polyvinyl chloride cable material. The polyvinyl chloride cable material comprises the following raw materials in parts by weight: 90-110 parts of polyvinyl chloride resin; 20 to 40 parts of trioctyl trimellitate; 10 to 30 parts of a halogen-free phosphorus-containing flame retardant; and 3-8 parts of a calcium-zinc stabilizer. The invention also relates to a preparation method of the polyvinyl chloride cable material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to a polyvinyl chloride cable material and a preparation method thereof. Background Art

[0002] This section provides background information related to the present application which does not necessarily constitute prior art.

[0003] The plastics used for the insulation layer and sheath of wires and cables are commonly known as cable materials. The existing polyvinyl chloride (PVC) cable materials are based on polyvinyl chloride resin, which is compounded with stabilizers (such as calcium zinc stabilizers, rare earth stabilizers, etc.), plasticizers (such as dioctyl phthalate, diisodecyl phthalate, dioctyl terephthalate, trioctyl trimellitate, etc.), inorganic fillers, lubricants and other additives.

[0004] Chlorophosphate plasticizers and chlorinated paraffin plasticizers are flame retardant, so they are called flame retardant plasticizers. Flame retardant plasticizers are added to PVC resin to make PVC cable materials with excellent flame retardant and transparent properties. However, since the main chain of PVC resin undergoes dehydrochlorination reaction to form a conjugated polyene structure at high temperature, a large amount of black smoke is produced during the combustion process. Chlorophosphate plasticizers and chlorinated paraffin plasticizers also have the problem of producing a large amount of black smoke during the heating process, resulting in the PVC cable material meeting the requirements in the flame retardant performance tests such as the limiting oxygen index and UL-94 flame retardant grade, but often not meeting the requirements in the flame retardant performance tests such as smoke density.

[0005] Although the mass percentage of chlorine in the PVC resin structure is as high as 56%, the flame retardancy of the PVC cable material is very good, and the limiting oxygen index (LOI) is greater than 45%, the addition of non-flame retardant plasticizers (such as phthalate plasticizers, terephthalate plasticizers, trimellitic acid triesters plasticizers, aliphatic dibasic acid ester plasticizers, linear polyester plasticizers, citrate plasticizers, and epoxy soybean oil plasticizers) will greatly reduce the limiting oxygen index of the PVC cable material, thereby reducing the flame retardancy of the PVC cable material. In order to solve the problem of reduced flame retardancy of the PVC cable material due to the addition of non-flame retardant plasticizers, the existing technical solution is to add inorganic flame retardants (such as antimony trioxide, magnesium hydroxide, aluminum hydroxide and other inorganic flame retardants) to solve the problem. Adding inorganic flame retardants can increase the limiting oxygen index of the PVC cable material to 30% or even higher, but because the refractive index of the existing inorganic flame retardants is greatly different from the refractive index of the PVC resin, the PVC cable material with the flame retardant added becomes opaque. Summary of the invention

[0006] The present invention aims to provide a PVC cable material which has excellent flame retardant performance, high visible light transmittance, low smoke density and excellent comprehensive mechanical properties.

[0007] The technical solution adopted by the present invention is: a PVC cable material, comprising the following raw materials in parts by weight:

[0008] PVC resin 90-110 parts;

[0009] 20-40 parts of trioctyl trimellitate;

[0010] 10-30 parts of halogen-free phosphorus-containing flame retardant;

[0011] Calcium zinc stabilizer 3-8 parts.

[0012] Wherein, the PVC resin is one or a combination of linear polyvinyl chloride resins with an average degree of polymerization between 1400 and 1600. The use of the polyvinyl chloride resin can simultaneously meet the requirements of mechanical properties of PVC cable materials and the flow properties required during processing. The PVC cable material prepared by adding trioctyl trimellitate to the linear PVC resin with a degree of polymerization within the above range has good elasticity. The inventor speculates that the reason is that the linear high-polymerization-degree PVC resin with a degree of polymerization within the above range has a large molecular weight and many physical crosslinking points (entanglement points) between molecules, which limits the relative movement between linear macromolecular chains and improves the resilience of PVC cable materials; at the same time, the physical crosslinking points (entanglement points) between such macromolecules constrain the movement of chain segments, making the stacking between molecules more compact, effectively improving the stability of the physical structure (shape) of the PVC cable material during combustion, improving the flame retardant properties of the PVC cable material, and improving its limiting oxygen index. The linear PVC resin with an average degree of polymerization of about 1500 is a more suitable choice, which can balance the elasticity, processing fluidity and flame retardant properties of the PVC cable material. If the degree of polymerization of PVC resin continues to increase, although the elasticity of PVC cable material can be appropriately improved, its processing flowability will deteriorate and the effect of improving flame retardant properties will no longer be significant.

[0013] Among them, trioctyl trimellitate is a non-flame retardant plasticizer. The PVC cable material prepared with this plasticizer has a lower smoke density, and the plasticizer is not easy to volatilize or migrate to the surface during processing and use.

[0014] Among them, the halogen-free phosphorus-containing flame retardant has strong heat resistance, acid and alkali resistance and hydrolysis resistance, and has a very low water absorption rate. It can be dissolved in organic solvents such as acetone, butanone, cyclohexanone and toluene, and the solubility rate is up to 50wt%. Therefore, it can be fully dispersed in the PVC resin system and has stable flame retardant performance. The halogen-free phosphorus-containing flame retardant in the present invention uses phosphorus-based flame retardants to promote polymer carbonization, plays a flame retardant role in the condensed phase, and has the advantages of high efficiency and low toxicity.

[0015] The preparation method of the halogen-free phosphorus-containing flame retardant described in the present invention is as follows:

[0016] Step 1, adding hydroxyethyllaurylamine, paraformaldehyde and tetrahydrofuran into a reaction container, stirring evenly and maintaining the temperature at 65-70° C. to obtain a first mixture in a transparent state;

[0017] Step 2, diethyl phosphite is added dropwise to the first mixture, and the mixture is reacted at a temperature of 65-70° C. for 8-9 hours. After the reaction is completed, the solvent is removed by rotary evaporation, and then the crude product is dissolved in chloroform, washed three times with 0.1 mol / L sodium hydroxide solution, and then dried, filtered and rotary evaporated to remove chloroform to obtain a first product;

[0018] Step 3, the first product is mixed with triethylamine and chloroform, stirred evenly and maintained at -5°C to obtain a second mixture, nicotinoyl chloride is added dropwise to the second mixture, the mixture is reacted for 9-10 hours, the temperature is raised to 5°C and the reaction is continued for 9-10 hours, after the reaction is completed, the triethylamine hydrochloride is filtered out, and the filtrate is washed with 0.1 mol / L sodium hydroxide solution, deionized water and saturated brine in sequence, and then dried over anhydrous sodium sulfate, filtered, and chloroform is removed by rotary evaporation to obtain a halogen-free phosphorus-containing flame retardant.

[0019] Wherein, in step 1, the molar ratio of hydroxyethyllaurylamine to paraformaldehyde is 1:1, and the amount of tetrahydrofuran added satisfies: the mass ratio of tetrahydrofuran to paraformaldehyde is not less than 3:2.

[0020] Wherein, in step 2, the molar ratio of hydroxyethyllaurylamine, paraformaldehyde and diethyl phosphite is 1:1:1.1. The reaction process of step 2 is as follows:

[0021]

[0022] Wherein, in step 3, the molar ratio of the first product to triethylamine is 1:2, the molar ratio of the first product to nicotinoyl chloride is 1:1, and the amount of chloroform added satisfies: the mass ratio of chloroform to triethylamine is not less than 15:2. The reaction process of step 3 is as follows:

[0023]

[0024] In one or more embodiments, without affecting the technical effects of the PVC cable material provided by the present invention, the PVC cable material also includes a flame retardant plasticizer such as tris (2-chloropropyl) phosphate, tris (2-chloroethyl) phosphate, etc., a resin processing aid such as an acrylic resin processing aid, etc., and a lubricant such as a low-density oxidized polyethylene wax, etc.

[0025] The method for preparing the PVC cable material provided by the present invention comprises the following steps:

[0026] Step 1: Add PVC resin into a hot-mix high-speed mixer, start the low-speed mixing mode to mix evenly, add calcium zinc stabilizer and continue to mix evenly;

[0027] Step 2, add part of trioctyl trimellitate, switch to high-speed mixing mode and mix evenly, when the temperature rises to 70-80°C, continue to add the remaining trioctyl trimellitate and mix evenly;

[0028] Step 3: After all the trioctyl trimellitate is completely absorbed by the PVC resin, add the halogen-free phosphorus-containing flame retardant and continue to mix evenly until the material temperature rises to 130-140°C and then extrude and granulate through a single screw extruder at 180-185°C to obtain a uniform and transparent PVC cable material.

[0029] The PVC cable material provided by the present invention can be used to prepare the insulation layer of wires and cables. In one or more embodiments, the PVC cable material is extruded by a cable extruder at 150-175° C. to obtain a transparent insulation layer of wires and cables.

[0030] Compared with the prior art, the present invention has at least the following beneficial effects:

[0031] 1. The PVC cable material provided by the present invention has excellent flame retardant properties, high visible light transmittance, low smoke density and excellent comprehensive mechanical properties. The PVC cable material meets the following requirements: UL-94 flame retardant grade meets V-0 grade, the limiting oxygen index range is 33%-35%, the smoke density grade is <70, the visible light transmittance is >90%, and the haze is <10%.

[0032] 2. The present invention improves the flame retardant properties of PVC cable materials by adding halogen-free phosphorus-containing flame retardants. While increasing the limiting oxygen index, the addition has no effect on the transparency of the PVC cable materials and has little effect on the smoke density of the PVC cable materials.

[0033] 3. The present invention adopts a linear polyvinyl chloride resin with an average degree of polymerization between 1400 and 1600, which absorbs plasticizer faster than PVC resin with an average degree of polymerization of 1000 to 1300, can shorten the pre-plasticization time in a high-speed mixer, and can meet the requirements that the PVC cable material has processability while having good elasticity, wear resistance and improved flame retardancy.

[0034] 4. The present invention uses trioctyl trimellitate as a plasticizer, while improving the limiting oxygen index, the PVC cable material can also maintain a low smoke density and a high visible light transmittance. It is generally believed in the existing knowledge that the PVC cable material prepared by mixing a plasticizer containing a benzene ring structure with PVC has a large smoke density during combustion and is not suitable for preparing flame-retardant and low-smoke PVC cable material, but it is unexpectedly found that the PVC cable material prepared by mixing trioctyl trimellitate with a linear polyvinyl chloride resin with an average degree of polymerization between 1400 and 1600 has a low smoke density during combustion.

[0035] The following describes the invention in conjunction with specific embodiments. DETAILED DESCRIPTION

[0036] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.

[0037] It should be noted that the performance test described in the embodiments of the present invention specifically includes the following:

[0038] 1. Limiting oxygen index determination: Use an oxygen index tester to test in accordance with GB / T 2406.2-2009 standard.

[0039] 2. Vertical combustion test (UL-94): According to the US UL-94 standard, the sample is placed vertically and the lower end of the sample is ignited with a flame of a specified height for 10 seconds. The burning time of the sample after the flame is removed is recorded. After the flame of the sample is extinguished, the flame is ignited again and the burning time is recorded. Repeat 5 times and the total cumulative burning time is used to determine the flame retardant grade.

[0040] 3. Smoke density test: Use a building material smoke density tester to test in accordance with GB / T 8627-2007 standard. Use liquefied petroleum gas with a pressure of 276KPa to burn the sample. Perform a total of three tests, each lasting 4 minutes. The SDR and MSD values ​​of the sample after three tests can be calculated based on the curve of the sample's light absorption rate and time.

[0041] 4. Transmittance and haze test: Tested in accordance with ASTM D 1003 standard, haze is expressed as the percentage of the scattered light flux to the light flux passing through the sample, while transmittance is the percentage of the light flux passing through the sample to its incident light flux. Generally speaking, the higher the transmittance and the lower the haze, the better the transparency.

[0042] 5. Mechanical properties test: The tensile strength test is carried out in accordance with GB / T528-1998 standard, and the elongation at break test is carried out in accordance with the national standard GB3923-83.

[0043] It should be noted that the preparation method of the halogen-free phosphorus-containing flame retardant described in the embodiments of the present invention is as follows:

[0044] Step 1, add hydroxyethyllaurylamine (CAS No.: 6961-46-2), paraformaldehyde (CAS No.: 30525-89-4) and tetrahydrofuran (CAS No.: 109-99-9) into a four-necked flask equipped with a mechanical stirrer, a thermometer, a dropping funnel and a condenser, the molar ratio of hydroxyethyllaurylamine to paraformaldehyde is 1:1, and the mass ratio of tetrahydrofuran to paraformaldehyde is 3:2, stir evenly and maintain at 68° C. to obtain a first mixture in a transparent state;

[0045] Step 2, diethyl phosphite (CAS number of diethyl phosphite is 762-04-9, and the molar ratio of hydroxyethyl laurylamine, polyformaldehyde and diethyl phosphite is 1:1:1.1) is added dropwise to the first mixture, and the mixture is reacted at a temperature of 68°C for 8 hours. After the reaction is completed, the solvent is removed by rotary evaporation, and then the crude product is dissolved in chloroform (CAS number: 67-66-3), washed three times with 0.1 mol / L sodium hydroxide solution, and then dried, filtered and rotary evaporated to remove chloroform to obtain a first product;

[0046] Step three, in a four-necked flask equipped with a drying tube, a dropping funnel and a mechanical stirrer, the first product, triethylamine (CAS number: 121-44-8) and chloroform (CAS number: 67-66-3) are added in sequence, the molar ratio of the first product to triethylamine is 1:2, and the mass ratio of chloroform to triethylamine is 15:2. Stir evenly and maintain at -5°C to obtain a second mixture, and nicotinoyl chloride (the CAS number of nicotinoyl chloride is 10400-19-8, and the molar ratio of the first product to nicotinoyl chloride is 1:1) is added dropwise to the second mixture. After reacting for 9 hours, the temperature is raised to 5°C and the reaction is continued for 9 hours. After the reaction is completed, the triethylamine hydrochloride is filtered out, and the filtrate is washed with 0.1 mol / L sodium hydroxide solution, deionized water and saturated brine in sequence, and then dried over anhydrous sodium sulfate, filtered, and rotary evaporated to remove chloroform to obtain a halogen-free phosphorus-containing flame retardant.

[0047] Examples 1-3 all provide a PVC cable material, and the specific composition ratio is shown in Table 1.

[0048] Comparative Examples 1-8 all provide a PVC cable material, and the specific composition ratios are shown in Table 2.

[0049] Table 1

[0050]

[0051] The preparation methods of the PVC cable materials provided in Examples 1-3 and Comparative Examples 1-8 both include the following steps:

[0052] Step 1: Add PVC resin into a hot-mix high-speed mixer, start the low-speed mixing mode (speed 450 rpm) to mix evenly, add stabilizer and continue to mix evenly;

[0053] Step 2: add half of the plasticizer, switch to high-speed mixing mode (speed 1000 rpm) and mix evenly. When the temperature rises to 70-80°C, continue to add the remaining half of the plasticizer and mix evenly.

[0054] Step 3: After all the plasticizers are completely absorbed by the PVC resin, add the flame retardant and continue to mix evenly until the material temperature rises to 140°C and then extrude and granulate through a single screw extruder at 185°C to obtain a uniform and transparent PVC cable material.

[0055] Table 2

[0056]

[0057] The performance test of the PVC cable materials provided in Examples 1-3 was performed, and the results are shown in Table 3. The performance test of the PVC cable materials provided in Comparative Examples 1-8 was performed, and the results are shown in Table 4.

[0058] Table 3

[0059] Performance Testing Example 1 Example 2 Example 3 Limiting oxygen index (%) 33.6 34.5 34.1 UL-94 test grade V-0 V-0 V-0 Smoke density level (%) 67.2 65.1 67.7 Maximum smoke density (%) 72.1 74.7 72.8 Visible light transmittance (%) 93.2 93.5 94.1 Haze(%) 7.2 7.5 7.7 Tensile strength(MPa) 24.7 25.3 24.5 Elongation at break (%) 365 421 397

[0060] Table 4

[0061] Performance Testing Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Comparative Example 7 Comparative Example 8 Limiting oxygen index (%) 30.5 35.4 31.2 31.6 29.8 30.3 23.4 30.5 UL-94 test grade V-0 V-0 V-0 V-0 V-0 V-0 flammable V-0 Smoke density level (%) 68.9 67.6 76.2 71.4 88.3 85.4 89.2 80.5 Maximum smoke density (%) 81.1 80.8 84.1 83.5 97.4 96.6 99.1 89.8 Visible light transmittance (%) 91.8 91.1 90.5 90.2 90.6 90.9 90.1 89.9 Haze(%) 9.7 10.1 11.1 10.6 11.7 9.5 9.9 12.1 Tensile strength(MPa) 22.1 21.8 21.2 24.8 23.8 22.7 22.5 21.9 Elongation at break (%) 298 315 289 288 312 328 315 308

[0062] According to the test results in Table 3 and Table 4, it can be judged that the PVC cable materials provided in Examples 1-3 can improve the limiting oxygen index while maintaining a low smoke density and a high visible light transmittance, and have excellent mechanical properties.

[0063] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0064] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A polyvinyl chloride cable material, characterized in that: The polyvinyl chloride cable material comprises the following raw materials in parts by weight: 90-110 parts of polyvinyl chloride resin; 20-40 parts of trioctyl trimellitate; 10-30 parts of halogen-free phosphorus-containing flame retardant; Calcium zinc stabilizer 3-8 parts; The polyvinyl chloride resin is one or a combination of linear polyvinyl chloride resins having an average degree of polymerization between 1400 and 1600; The preparation method of the halogen-free phosphorus-containing flame retardant is as follows: Step 1, adding hydroxyethyllaurylamine, paraformaldehyde and tetrahydrofuran into a reaction container, stirring evenly and maintaining the temperature at 65-70° C. to obtain a first mixture in a transparent state; Step 2, diethyl phosphite is added dropwise to the first mixture, and the mixture is reacted at a temperature of 65-70° C. for 8-9 hours. After the reaction is completed, the solvent is removed by rotary evaporation, and then the crude product is dissolved in chloroform, washed three times with 0.1 mol / L sodium hydroxide solution, and then dried, filtered and rotary evaporated to remove chloroform to obtain a first product; Step 3, mixing the first product with triethylamine and chloroform, stirring evenly and maintaining at -5°C to obtain a second mixture, adding nicotinyl chloride dropwise to the second mixture, reacting for 9-10 hours, heating to 5°C and continuing to react for 9-10 hours, after the reaction is completed, filtering to remove triethylamine hydrochloride, washing the filtrate with 0.1 mol / L sodium hydroxide solution, deionized water and saturated brine in sequence, and then drying with anhydrous sodium sulfate, filtering, and rotary evaporating to remove chloroform to obtain the halogen-free phosphorus-containing flame retardant.

2. The polyvinyl chloride cable material according to claim 1, characterized in that: In the step 1, the molar ratio of hydroxyethyllaurylamine to paraformaldehyde is 1:1, and the amount of tetrahydrofuran added satisfies that the mass ratio of tetrahydrofuran to paraformaldehyde is not less than 3:

2.

3. The polyvinyl chloride cable material according to claim 2, characterized in that: In the step 2, the molar ratio of hydroxyethyllaurylamine, paraformaldehyde and diethyl phosphite is 1:1:1.

1.

4. The polyvinyl chloride cable material according to claim 3, characterized in that: In the step 3, the molar ratio of the first product to triethylamine is 1:2, the molar ratio of the first product to nicotinoyl chloride is 1:1, and the amount of chloroform added satisfies that the mass ratio of chloroform to triethylamine is not less than 15:

2.

5. A method for preparing the polyvinyl chloride cable material according to claim 4, characterized in that: The method comprises the following steps: Step 1: Add polyvinyl chloride resin into a hot-mix high-speed mixer, start the low-speed mixing mode to mix evenly, add calcium zinc stabilizer and continue to mix evenly; Step 2, add part of trioctyl trimellitate, switch to high-speed mixing mode and mix evenly, when the temperature rises to 70-80°C, continue to add the remaining trioctyl trimellitate and mix evenly; Step three, when all the trioctyl trimellitate is completely absorbed by the polyvinyl chloride resin, add the halogen-free phosphorus-containing flame retardant and continue to mix evenly until the material temperature rises to 130-140° C., and then extrude and granulate through a single screw extruder at 180-185° C. to obtain the polyvinyl chloride cable material.