Composition for degradable cup cover, preparation method of composition and cup cover

By adding glass fiber and modified bamboo fiber to polylactic acid materials and using the twin-screw extrusion mechanism to prepare technology, the problem of insufficient mechanical strength and heat resistance of polylactic acid materials in thin-walled products is solved, and rapid degradation and Combining high heat resistance and adding antibacterial agents to the material ensures the environmental friendliness and safety of the product.

CN118956124AActive Publication Date: 2024-11-15PANAN COUNTY XINYUAN NEW MATERIAL TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411225634.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-15
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

Existing polylactic acid materials are difficult to meet the requirements of rapid degradation, high mechanical strength and heat resistance at the same time, especially in thin-walled products such as milk tea cup lids.

Method used

After mixing lubricant, compatible agent, toughener, first polylactic acid and second polylactic acid by using a twin screw extruder, glass fiber and modified bamboo fiber are added, and the degradable cup lid is prepared by extrusion granulation. The composition uses polylactic acid with different weight average molecular weights, modified bamboo fibers and glass fibers to improve the flowability, mechanical properties and heat resistance of the material, and loads antibacterial agents in the bamboo fibers.

Benefits of technology

The comprehensive effect of rapid degradation of the degradable cup lid material, high mechanical strength and good heat resistance is achieved, ensuring that the product is not prone to deform under high temperature conditions and has antibacterial and antibacterial properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005024430600000141
    Figure BDA0005024430600000141
  • Figure BDA0005024430600000142
    Figure BDA0005024430600000142
Patent Text Reader

Abstract

The invention provides a composition for a degradable cup cover, a preparation method of the composition and the cup cover. The preparation method comprises the following steps: feeding a lubricant, a compatilizer, a flexibilizer, first polylactic acid and second polylactic acid into a double-screw extruder, and uniformly mixing and stirring; adding glass fibers and modified bamboo fibers into the double-screw extruder according to the addition amount of second polylactic acid, uniformly mixing and stirring again, and co-extruding and granulating to obtain the composition for the degradable cup cover; wherein the weight-average molecular weight of the first polylactic acid ranges from 5000 to 10000, and the weight-average molecular weight of the second polylactic acid ranges from 250000 to 300000; the modified bamboo fiber is subjected to calcium carbonate surface modification and is loaded with an antibacterial agent. The modified bamboo fiber is subjected to calcium carbonate surface modification and is loaded with an antibacterial agent. The composition for the degradable cup cover, which is obtained by the preparation method disclosed by the invention, has good degradability, mechanical property and heat resistance, and can resist and inhibit bacteria.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of degradable high molecular polymers, and in particular to a composition for a degradable cup cover, a preparation method thereof, and a cup cover. Background Art

[0002] Polylactic acid (PLA), also known as polylactide, is a new type of biodegradable material and belongs to thermoplastic aliphatic polyester polymers. The main raw material source of polylactic acid is renewable plant resources, such as corn, sugar cane, cassava, etc. These plants are rich in starch, which is finally converted into lactic acid through starch extraction, saccharification, fermentation and other steps, and then synthesized into polylactic acid through chemical synthesis. Polylactic acid has good biocompatibility and biodegradability. After use, it can be completely degraded by microorganisms in nature, and finally produces carbon dioxide and water, without polluting the environment. Due to the good transparency and processability of polylactic acid, it is widely used in food packaging, biodegradable plastic bags, food containers and other fields.

[0003] In recent years, people's consumption demand for milk tea, coffee and other beverages has continued to increase, and the market demand for degradable disposable beverage containers has also continued to expand. Environmentally friendly polylactic acid is the first choice for manufacturing such products.

[0004] In order to further improve the degradability of polylactic acid materials, the prior art generally adds natural substances such as plant fibers and starch in the preparation process of polylactic acid materials. In addition, since polylactic acid materials are brittle, have a low softening point, and have poor heat resistance, the prior art also adds inorganic fillers such as talcum powder, calcium carbonate, and montmorillonite to improve the mechanical strength and heat resistance of polylactic acid materials.

[0005] In particular, for products such as milk tea cup lids, the wall thickness is small, which requires high material fluidity. In addition, the brittleness of the material will increase significantly when the wall thickness is thin. At the same time, when holding food, disposable tableware must have a certain heat resistance. Existing polylactic acid biodegradable materials are difficult to simultaneously meet the requirements of rapid degradation, high strength, and heat resistance. Summary of the invention

[0006] The problem solved by the invention is how to provide a polylactic acid material which can be rapidly degraded, has high mechanical strength and good heat resistance.

[0007] In order to solve at least one of the above problems, the present invention provides a method for preparing a composition for a degradable cup cover, the preparation method comprising:

[0008] S100, feeding the lubricant, the compatibilizer, the toughening agent, the first polylactic acid and the second polylactic acid into a twin-screw extruder and mixing and stirring them uniformly according to the mass ratio of lubricant: compatibilizer: toughening agent: first polylactic acid: second polylactic acid = (1-2): (6-8): (6-8): (8-10): 100;

[0009] S200, adding glass fiber and modified bamboo fiber to a twin-screw extruder according to the mass ratio of glass fiber: modified bamboo fiber: second polylactic acid = (5-10): (15-20): 100 and the amount of the second polylactic acid added in S100, mixing and stirring again, and extruding and granulating together to obtain a composition for a degradable cup cover;

[0010] The weight average molecular weight of the first polylactic acid is 5000 to 10000, and the weight average molecular weight of the second polylactic acid is 250000 to 300000; the surface of the modified bamboo fiber is modified by calcium carbonate and loaded with an antibacterial agent. The surface of the modified bamboo fiber is modified by calcium carbonate and loaded with an antibacterial agent.

[0011] In any of the above technical solutions, the lubricant includes at least one of fatty acid esters, fatty acid amides and polyethylene wax, or a combination thereof; and / or the compatibilizer includes at least one of maleic anhydride, methyl diphenyl diisocyanate, lysine triisocyanate, lysine diisocyanate, and glycidyl methacrylate, or a combination thereof; and / or the toughening agent includes at least one of polybutylene succinate, polybutylene succinate adipate, polycaprolactone, and polybutylene adipate terephthalate, or a combination thereof; and / or the glass fiber includes at least one of silicate glass fiber, aluminosilicate glass fiber, alkali metal aluminosilicate glass fiber, and alkaline earth metal aluminosilicate glass fiber, or a combination thereof.

[0012] In any of the above technical solutions, the extrusion granulation temperature of the twin-screw extruder in S200 is: first section: 160°C to 170°C, second section: 180°C to 190°C, third section: 190°C to 200°C, fourth section: 160°C to 170°C, fifth section: 140°C to 150°C.

[0013] In any of the above technical solutions, the antibacterial agent is an inorganic non-metallic oxide antibacterial agent.

[0014] In any of the above technical solutions, the steps of preparing the modified bamboo fiber include:

[0015] S110, using a crusher to crush the bamboo fibers into bamboo fiber powder of target particle size;

[0016] S120, soaking the bamboo fiber powder in hydrogen peroxide, adding an acetic acid aqueous solution of the same volume as the hydrogen peroxide after the soaking is completed and stirring simultaneously, leaving the mixture to stand after the addition is completed, filtering, washing, and drying the bamboo fiber powder;

[0017] S130, uniformly dispersing the bamboo fiber powder obtained in S120 by ultrasonic dispersion in a calcium chloride aqueous solution, and dripping a sodium hydroxide aqueous solution until the pH reaches 11-12, to obtain a first mixture;

[0018] S140, placing the first mixture in a closed reactor for aging, first evacuating the reactor, then introducing a gas including carbon dioxide into the reactor, stirring the first mixture under pressure to allow the first mixture to react with the carbon dioxide, stopping the introduction of gas after the reaction is completed, releasing the pressure, extracting the solids, filtering, washing, and drying, and obtaining modified bamboo fiber.

[0019] In any of the above technical solutions, the target particle size of the bamboo fiber powder in S110 is 400 to 600 mesh; and / or the concentration of hydrogen peroxide in S120 is 20% to 25%; and / or the concentration of the acetic acid aqueous solution in S120 is 14% to 18%; and / or the soaking time in S120 is 2h to 3h, and the standing time is 20min to 40min; and / or the concentration of the calcium chloride aqueous solution in S130 is 10wt% to 20wt%; and / or the concentration of the sodium hydroxide aqueous solution in S130 is 8wt% to 12wt%; and / or the aging time in S140 is 12h to 18h; and / or the pressurization condition in S140 is 4MPa to 8MPa; and / or the stirring rate in S140 is 600r / min to 800r / min, and the stirring time is 2h to 5h.

[0020] In any of the above technical solutions, after S140, the preparation step of the modified bamboo fiber further includes:

[0021] S150, mixing carboxymethyl cellulose and starch in water, and placing in a water bath at 75° C. to 80° C., keeping warm and stirring for 20 to 40 minutes to obtain gelatinized starch;

[0022] S160, mixing maleic anhydride, ammonium persulfate, acrylic acid and acrylamide to obtain a second mixture;

[0023] S170, lowering the temperature of the water bath to 50° C. to 60° C., adding the second mixture to the water bath according to the amount of starch in S150, and continuing to keep warm and stir for 1 to 2 hours to obtain modified starch;

[0024] S180, mixing zinc chloride, the modified starch obtained in S170 and the modified bamboo fiber obtained in S140 in water, stirring evenly and letting stand for 4 to 6 hours, adding 8wt% to 12wt% sodium hydroxide aqueous solution until the pH reaches 11-12, letting stand again for 4 to 6 hours, filtering, washing and drying to obtain bamboo fiber powder loaded with an antibacterial agent.

[0025] In any of the above technical solutions, in S150, by mass ratio, carboxymethyl cellulose: starch: water = (2-4): (15-25): 100; and / or in S160, by mass ratio, maleic anhydride: ammonium persulfate: acrylic acid: acrylamide = (0.2-0.4): (1-1.5): (30-40): 100; and / or in S170, by mass ratio, the second mixture: starch = (10-20): 100; and / or in S180, by mass ratio, zinc chloride: modified starch: modified bamboo fiber: water = (6-8): (10-20): (20-30): 100.

[0026] The present invention also provides a degradable composition for cup covers, which is obtained by using the preparation method of any of the above technical solutions.

[0027] The present invention also provides a cup cover, which is manufactured using the degradable composition for cup covers obtained by the preparation method of any of the above technical solutions.

[0028] Beneficial Effects

[0029] The present invention provides a method for preparing a composition for a degradable cup cover, wherein the preparation method uses a lubricant, a compatibilizer, a toughening agent, a first polylactic acid, a second polylactic acid, glass fiber and modified bamboo fiber as raw materials. The method firstly sends the lubricant, the compatibilizer, the toughening agent, the first polylactic acid and the second polylactic acid into a twin-screw extruder for mixing and stirring, and after the above raw materials are evenly mixed, glass fiber and modified bamboo fiber are added, and the mixing is continued, and finally extrusion granulation is performed to obtain a composition for a degradable cup cover. The difference between the first polylactic acid and the second polylactic acid is that the weight average molecular weight of the first polylactic acid is 5000 to 10000, and the weight average molecular weight of the second polylactic acid is 250000 to 300000. Since the present invention adds two kinds of polylactic acid with different weight average molecular weights, the second polylactic acid with large weight average molecular weight is used as the main raw material, and the first polylactic acid with small weight average molecular weight is used as a flow promoter, so that when the composition for degradable cup cover is used to prepare products with smaller wall thickness, its melt flow rate can meet the processing requirements of thin-wall injection molding, and ensure the processing accuracy of the product. Glass fiber has good mechanical properties, excellent mechanical properties, good chemical stability and good heat resistance. Therefore, the addition of glass fiber can improve the mechanical properties and heat resistance of the composition for degradable cup cover, so that it is not easy to be deformed and damaged by high temperature when used as a disposable beverage container for hot drinks. Bamboo fiber, as a natural plant fiber, can further improve the degradability of polylactic acid polymer materials and improve their environmental friendliness. In summary, the present invention can provide a composition for degradable cup cover that can be quickly degraded, has high mechanical strength and good heat resistance through the above technical scheme. In addition, considering that the mechanical strength of bamboo fiber itself is poor, and as a natural plant fiber, it is difficult to be compatible with polymers and difficult to be evenly dispersed in polymers, the bamboo fiber used in the present invention has been surface-modified with calcium carbonate. Calcium carbonate can improve the mechanical strength of bamboo fiber on the one hand, and on the other hand, it can also improve the compatibility between bamboo fiber and polymer. Finally, considering the antibacterial and mildew-proof needs of the degradable cup cover composition, the present invention loads an antibacterial agent in the bamboo fiber to ensure that the degradable cup cover composition has good degradability, mechanical properties and heat resistance, and can be antibacterial and antibacterial. DETAILED DESCRIPTION

[0030] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the following is a detailed description of the specific embodiments of the present invention.

[0031] Unless otherwise specified, the reagents and raw materials used in the present invention can be purchased through commercial channels. The experimental methods in the following examples without specifying specific conditions are selected according to conventional methods and conditions, or according to the product specifications.

[0032] Polylactic acid is a green renewable resource with good biodegradability and biocompatibility, and is an ideal degradable polymer material. The present invention provides a composition for a degradable cup cover and a preparation method thereof. The purpose of the present invention is to provide a polylactic acid-based degradable cup cover composition that has good degradability, mechanical properties, and heat resistance, and can be antibacterial and bacteriostatic. The preparation method of the degradable cup cover composition of the present invention is as follows:

[0033] S100, feeding the lubricant, the compatibilizer, the toughening agent, the first polylactic acid and the second polylactic acid into a twin-screw extruder and mixing and stirring them uniformly according to the mass ratio of lubricant: compatibilizer: toughening agent: first polylactic acid: second polylactic acid = (1-2): (6-8): (6-8): (8-10): 100;

[0034] S200, adding glass fiber and modified bamboo fiber to a twin-screw extruder according to the mass ratio of glass fiber: modified bamboo fiber: second polylactic acid = (5-10): (15-20): 100 and the amount of the second polylactic acid added in S100, mixing and stirring again, and extruding and granulating together to obtain a composition for a degradable cup cover;

[0035] The weight average molecular weight of the first polylactic acid is 250,000 to 300,000, and the weight average molecular weight of the second polylactic acid is 5,000 to 10,000. The modified bamboo fiber is surface-modified with calcium carbonate and loaded with an antibacterial agent.

[0036] In the above steps, the role of each component is as follows. Lubricants can significantly reduce the friction between polymer materials, making the materials smoother during mixing, extrusion, injection molding, etc., reducing energy loss and equipment wear. In a specific embodiment of the present invention, the lubricant includes at least one of fatty acid esters, fatty acid amides and polyethylene wax or a combination thereof. Preferably, the lubricant used in the present invention is butyl stearate. In a polymer blend system, a compatibilizer can effectively reduce the particle size of the dispersed phase, making the dispersed phase more evenly distributed in the continuous phase, thereby improving the mechanical properties and processing properties of the material. In a specific embodiment of the present invention, a compatibilizer includes at least one of maleic anhydride, methyl diphenyl diisocyanate, lysine triisocyanate, lysine diisocyanate, and glycidyl methacrylate or a combination thereof. Preferably, the compatibilizer used in the present invention is maleic anhydride. Tougheners can reduce the brittleness of polymers, improve their toughness, and improve the processing properties of polymers. In a specific embodiment of the present invention, the toughening agent includes at least one of polybutylene succinate, polybutylene succinate adipate, polycaprolactone, and polybutylene adipate terephthalate or a combination thereof. Preferably, the toughening agent used in the present invention is polybutylene succinate. Glass fiber has the characteristics of high strength and high modulus. Adding it to a polymer can significantly improve the mechanical properties of the composite material such as tensile strength, flexural strength, and impact strength. This makes the glass fiber reinforced polymer composite material more stable when subjected to external force and is not prone to breakage or deformation. In a specific embodiment of the present invention, the glass fiber includes at least one of silicate glass fiber, aluminosilicate glass fiber, alkali metal aluminosilicate glass fiber, and alkaline earth metal aluminosilicate glass fiber or a combination thereof. Preferably, the glass fiber used in the present invention is aluminosilicate glass fiber. Bamboo fiber itself is biodegradable, and after being combined with a degradable polymer, it can further promote the degradation performance of the composite material. In the degradation process, bamboo fiber will be the first to degrade, providing channels and space for the degradation of the polymer, thereby accelerating the degradation process of the entire composite material.

[0037] The present invention adopts a twin-screw extruder to prepare a composition for a degradable cup lid by extrusion granulation. The process of preparing polylactic acid materials by extrusion granulation belongs to the prior art. Those skilled in the art are capable of selecting and adjusting the equipment and process parameters used for extrusion granulation according to actual needs, and the present invention will not elaborate on it. Preferably, the extrusion granulation temperature of the twin-screw extruder in S200 is: first section: 160°C to 170°C, second section: 180°C to 190°C, third section: 190°C to 200°C, fourth section: 160°C to 170°C, fifth section: 140°C to 150°C.

[0038] Since the present invention adds two polylactic acids with different weight average molecular weights, the second polylactic acid with a large weight average molecular weight is used as the main raw material, and the first polylactic acid with a small weight average molecular weight is used as a flow promoter, the melt flow rate of the composition for the degradable cup cover can meet the processing requirements of thin-wall injection molding when it is used to prepare products with a smaller wall thickness, thereby ensuring the processing accuracy of the product.

[0039] The modified bamboo fiber of the present invention is surface-modified by calcium carbonate, and its purpose is to improve the mechanical strength of the bamboo fiber. Specifically, although bamboo fiber, as a natural plant fiber, can improve the degradability of polylactic acid materials, its mechanical properties need to be further improved. Calcium carbonate, as an inorganic material, can improve the mechanical properties of bamboo fiber. In addition, the prior art including CN111516073A, CN106182298A, etc. also reports that calcium carbonate is used as a filler and mixed with plant fiber powder to fill resin, which can prevent crack propagation of resin materials and accelerate the dissipation of impact energy through interface plastic deformation, thereby achieving the purpose of enhancing the strength of resin materials.

[0040] Therefore, the present invention selects calcium carbonate to modify the bamboo fiber. The preparation steps of the modified bamboo fiber include:

[0041] S110, using a crusher to crush the bamboo fibers into bamboo fiber powder of target particle size;

[0042] S120, soaking the bamboo fiber powder in hydrogen peroxide, adding an acetic acid aqueous solution of the same volume as the hydrogen peroxide after the soaking is completed and stirring simultaneously, leaving the mixture to stand after the addition is completed, filtering, washing, and drying the bamboo fiber powder;

[0043] S130, uniformly dispersing the bamboo fiber powder obtained in S120 by ultrasonic dispersion in a calcium chloride aqueous solution, and dripping a sodium hydroxide aqueous solution until the pH reaches 11-12, to obtain a first mixture;

[0044] S140, placing the first mixture in a closed reactor for aging, first evacuating the reactor, then introducing a gas including carbon dioxide into the reactor, stirring the first mixture under pressure to allow the first mixture to react with the carbon dioxide, stopping the introduction of gas after the reaction is completed, releasing the pressure, extracting the solids, filtering, washing, and drying, and obtaining modified bamboo fiber;

[0045] S150, mixing carboxymethyl cellulose and starch in water, and placing in a water bath at 75° C. to 80° C., keeping warm and stirring for 20 to 40 minutes to obtain gelatinized starch;

[0046] S160, mixing maleic anhydride, ammonium persulfate, acrylic acid and acrylamide to obtain a second mixture;

[0047] S170, lowering the temperature of the water bath to 50° C. to 60° C., adding the second mixture to the water bath according to the amount of starch in S150, and continuing to keep warm and stir for 1 to 2 hours to obtain modified starch;

[0048] S180, mixing zinc chloride, the modified starch obtained in S170 and the modified bamboo fiber obtained in S140 in water, stirring evenly and letting stand for 4 to 6 hours, adding 8wt% to 12wt% sodium hydroxide aqueous solution until the pH reaches 11-12, letting stand again for 4 to 6 hours, filtering, washing and drying to obtain bamboo fiber powder loaded with an antibacterial agent.

[0049] In some embodiments of the present invention, the target particle size of the bamboo fiber powder in S110 is 400 mesh to 600 mesh. Those skilled in the art can select and adjust the particle size of the bamboo fiber according to actual needs.

[0050] In some embodiments of the present invention, the concentration of hydrogen peroxide in S120 is 20% to 25%, the concentration of acetic acid aqueous solution in S120 is 14% to 18%, the concentration of calcium chloride aqueous solution in S130 is 10wt% to 20wt%, and the concentration of sodium hydroxide aqueous solution in S130 is 8wt% to 12wt%.

[0051] Preferably, the concentration of hydrogen peroxide in S120 is 20%, the concentration of acetic acid aqueous solution in S120 is 15%, the concentration of calcium chloride aqueous solution in S130 is 12wt%, and the concentration of sodium hydroxide aqueous solution in S130 is 10wt%.

[0052] In some embodiments of the present invention, the immersion time in S120 is 2h to 3h, the standing time is 20min to 40min, the aging time in S140 is 12h to 18h, the pressurization condition in S140 is 4MPa to 8MPa, the stirring rate in S140 is 600r / min to 800r / min, and the stirring time is 2h to 5h.

[0053] Preferably, the soaking time in S120 is 2.5 h, the standing time is 30 min, the aging time in S140 is 15 h, the pressurization condition in S140 is 6 MPa, the stirring rate in S140 is 600 r / min, and the stirring time is 3 h.

[0054] In some embodiments of the present invention, in S150, by mass ratio, carboxymethyl cellulose: starch: water = (2-4): (15-25): 100; in S160, by mass ratio, maleic anhydride: ammonium persulfate: acrylic acid: acrylamide = (0.2-0.4): (1-1.5): (30-40): 100; in S170, by mass ratio, the second mixture: starch = (10-20): 100; in S180, by mass ratio, zinc chloride: modified starch: modified bamboo fiber: water = (6-8): (10-20): (20-30) 100.

[0055] Preferably, in S150, by mass ratio, carboxymethyl cellulose: starch: water = 2:20:100; in S160, by mass ratio, maleic anhydride: ammonium persulfate: acrylic acid: acrylamide = 0.2:1:30:100; in S170, by mass ratio, the second mixture: starch = 15:100; in S180, by mass ratio, zinc chloride: modified starch: modified bamboo fiber: water = 6:10:30:100.

[0056] One of the purposes of the above steps is to load the bamboo fiber with calcium carbonate uniformly and in large quantities. Specifically, the present invention first crushes the bamboo fiber into powder through S110, and then cleans and removes impurities from the bamboo fiber powder through S120. By soaking the bamboo fiber powder in hydrogen peroxide, the bamboo fiber can be separated and the purpose of bleaching can be achieved, thereby ensuring that the whiteness and appearance of the bamboo fiber meet the processing requirements. Furthermore, by dripping acetic acid aqueous solution into the hydrogen peroxide without bamboo fiber, acetic acid and hydrogen peroxide can be generated to generate active oxygen, and the active oxygen is used to further clean the bamboo fiber, remove bacteria in the bamboo fiber, and effectively prevent it from getting moldy during use.

[0057] In S130, by ultrasonically dispersing bamboo fiber powder in calcium chloride aqueous solution uniformly and dripping sodium hydroxide aqueous solution, calcium ions can be made to generate calcium hydroxide under alkaline conditions. The cell structure of bamboo fiber causes it to produce a capillary effect, so that the calcium ions in the calcium chloride aqueous solution penetrate the plant cells, fully enter and occupy the cell structure of bamboo fiber, and are deposited on at least part of the interior and surface of bamboo fiber powder. Under alkaline conditions, calcium ions and hydroxyls are combined, and calcium hydroxide enters between the cell gaps and the cell cavity of bamboo fiber, and evenly and massively loads calcium hydroxide on at least part of the interior and surface of bamboo fiber powder. Then, by S140, calcium hydroxide in bamboo fiber powder can be made to react with carbon dioxide under high pressure conditions, and calcium hydroxide reacts with carbon dioxide to generate calcium carbonate, and calcium carbonate precipitation is coated on at least part of the interior and surface of bamboo fiber powder, so that the mechanical properties of bamboo fiber can be improved.

[0058] Furthermore, the present invention adopts zinc oxide as an inorganic non-metallic oxide antibacterial agent, and loads it on bamboo fiber, in order to improve the antibacterial and antibacterial properties of the degradable cup cover composition. The degradable cup cover composition of the present invention is particularly suitable for use as a cup cover for beverages such as coffee and milk tea. The consumer group of such beverages is constantly expanding, and some consumers will put the remaining unfinished beverages into the refrigerator for storage after purchasing beverages such as coffee and milk tea. Such beverages contain more sugar, and after being placed for a long time (especially in a complex environment such as a refrigerator where harmful bacteria may exist), it is easy to breed bacteria, affecting food safety. Therefore, the present invention adopts an inorganic non-metallic oxide antibacterial agent to give the degradable cup cover composition better antibacterial and antibacterial properties, making it more suitable for making cup covers for beverages such as coffee and milk tea.

[0059] Metal ions such as zinc ions, titanium ions, silver ions, and strontium ions all have good long-term antibacterial and antimicrobial effects. The oxides of the above metal ions are stable, safe and effective, and are widely used as antibacterial agents for food packaging materials. The present invention selects zinc oxide as an antibacterial agent. When zinc oxide comes into contact with bacteria, zinc ions are released. These zinc ions have redox properties and can bind to bacterial cell membranes and membrane proteins, and react with functional groups such as sulfhydryl, carboxyl, and hydroxyl groups in their structures, thereby destroying the structure of bacteria. After entering bacterial cells, zinc ions can also destroy enzymes in the electron transfer system and react with DNA to achieve the purpose of antibacterial.

[0060] Nano zinc fungicide has poor dispersibility in polymer materials and is easy to agglomerate, thereby affecting its bactericidal efficiency. Therefore, the present invention uniformly loads zinc ions in starch and bamboo fiber. To achieve this purpose, the present invention first prepares a modified starch in a gel state that can adsorb metal ions, and then uses the modified starch and zinc chloride to mix with bamboo fiber, so that the zinc ions are adsorbed by the modified starch and mixed with the bamboo fiber. Specifically, the present invention gelatinizes the starch through S150, so that the starch particles absorb water and swell and destroy their crystal structure, thereby breaking the original morphological structure of the starch particles, making it more compatible with bamboo fiber. In addition, the gelatinized starch is easier to be decomposed by microorganisms, accelerating the degradation process of polylactic acid plastics. Acrylic acid and acrylamide, as monomers, can undergo polymerization reaction at a suitable temperature (50°C to 60°C) under the action of initiator ammonium persulfate and cross-linking agent maleic anhydride to generate acrylic copolymers. By mixing starch gelatinized into a colloidal state with maleic anhydride, ammonium persulfate, acrylic acid and acrylamide, and reacting at a temperature of 50°C to 60°C, starch modified by acrylic acid copolymer can be obtained. There are a large number of hydroxyl groups and phosphate groups with obvious cationic properties in the starch molecule itself, and the copolymerization of acrylic acid and acrylamide generates anionic acrylic acid copolymers, and -COOH groups and -COONa groups are contained therein. This enables the starch modified by the acrylic acid copolymer to electrostatically adsorb metal cations and load a larger amount of metal ions. Therefore, the present invention prepares starch modified by acrylic acid copolymer, and mixes it with zinc chloride and modified bamboo fiber, so that the starch uniformly and massively adsorbs metal zinc ions, and by dripping sodium hydroxide aqueous solution, zinc hydroxide is deposited and loaded in starch and bamboo fiber, and bamboo fiber loaded with antibacterial agent is obtained. Furthermore, in the process of blending and extruding bamboo fiber and polylactic acid, the high temperature above 150°C oxidizes zinc hydroxide into zinc oxide, and evenly and stably disperses it in bamboo fiber and starch, playing a long-term antibacterial and antibacterial effect.

[0061] Example 1

[0062] In this embodiment, a modified bamboo fiber sample was prepared, and its preparation process was as follows:

[0063] S1. Use a crusher to crush the bamboo fiber into bamboo fiber powder of 400 to 600 meshes;

[0064] S2. Soak the bamboo fiber powder in 20% hydrogen peroxide for 2.5 hours. After soaking, add 15% acetic acid aqueous solution with the same volume as the hydrogen peroxide and stir simultaneously. After the addition is completed, let it stand for 30 minutes, filter the solids, wash with deionized water for 2-3 times until there is no smell, and dry it with infrared drying to obtain bamboo fiber sample 1.

[0065] Example 2

[0066] In this example, the bamboo fiber sample obtained in Example 1 is further processed in the following manner:

[0067] S1. After the bamboo fiber powder obtained in Example 1 is uniformly dispersed by ultrasonic in a 12 wt % calcium chloride aqueous solution at a mass ratio of bamboo fiber powder to calcium chloride aqueous solution = 20:100, a 10 wt % sodium hydroxide aqueous solution is added dropwise until the pH reaches 11-12 to obtain a first mixture;

[0068] S2. The first mixture is placed in a closed reactor for aging for 15 hours, and then the reactor is evacuated, and then gas is introduced into the reactor, wherein the gas includes a mixed gas of carbon dioxide and nitrogen in a volume ratio of 1:9. After the pressure of the mixed gas reaches 6 MPa, the first mixture is stirred at a rate of 600 r / min to allow the first mixture to react with the carbon dioxide. After maintaining the pressure for 3 hours, the gas introduction is stopped, the pressure is released, and the solids are extracted for filtration, washed with deionized water 2-3 times, and infrared dried to obtain bamboo fiber sample 2.

[0069] Example 3

[0070] In this example, the modified bamboo fiber sample obtained in Example 2 is further processed in the following manner:

[0071] S1. Mix carboxymethyl cellulose and starch in water in a mass ratio of carboxymethyl cellulose: starch: water = 2:20:100, and keep stirring in a water bath at 75° C. for 20 min to obtain gelatinized starch;

[0072] S2, mixing maleic anhydride, ammonium persulfate, acrylic acid and acrylamide in a mass ratio of maleic anhydride: ammonium persulfate: acrylic acid: acrylamide = 0.2:1:30:100 to obtain a second mixture;

[0073] S3, lowering the temperature of the water bath to 55°C, adding the second mixture into the water bath immediately after the second mixture is mixed according to the mass ratio of the second mixture to starch = 15:100, and continuing to keep warm and stir for 1.5 hours. After the stirring is completed, extracting the solid matter to obtain a modified starch in a colloidal state;

[0074] S4. According to the mass ratio of zinc chloride: modified starch: modified bamboo fiber: water = 6:10:30:100, zinc chloride, the modified starch obtained in S3 and the bamboo fiber of Example 2 are mixed in water, stirred evenly and allowed to stand for 6 hours, 10 wt % sodium hydroxide aqueous solution is added dropwise until the pH reaches 11-12, and allowed to stand for 4 hours again. The mixture is filtered, washed with deionized water 2-3 times, and infrared dried to obtain bamboo fiber sample 3.

[0075] Example 4

[0076] In this example, the modified bamboo fiber sample obtained in Example 2 is further processed in the following manner:

[0077] S1. Mix carboxymethyl cellulose and starch in water in a mass ratio of carboxymethyl cellulose: starch: water = 2:20:100, and keep stirring in a water bath at 75° C. for 20 min to obtain gelatinized starch;

[0078] S2. According to the mass ratio of zinc chloride: gelatinized starch: modified bamboo fiber: water = 6:10:30:100, zinc chloride, gelatinized starch obtained in S1 and bamboo fiber of Example 2 are mixed in water, stirred evenly and allowed to stand for 6 hours, 10 wt % sodium hydroxide aqueous solution is added dropwise until the pH reaches 11-12, allowed to stand again for 4 hours, filtered, washed with deionized water 2-3 times, and infrared dried to obtain bamboo fiber sample 4.

[0079] Example 5

[0080] In this embodiment, a series of composition samples 1-8 for degradable cup lids are prepared. The raw material ratios of the composition samples 1-8 are listed in Table 1. The preparation process is as follows:

[0081] S1, feeding butyl stearate, maleic anhydride, polybutylene succinate, a first polylactic acid having a weight average molecular weight of 5000 to 10000 and a second polylactic acid having a weight average molecular weight of 250000 to 300000 into a twin-screw extruder and mixing and stirring uniformly;

[0082] S2. According to the amount of the second polylactic acid added in S1, add glass fiber and modified bamboo fiber to the twin-screw extruder, mix and stir evenly again, and extrude and granulate together to obtain a composition for a degradable cup lid; wherein, the temperature of the first stage of extrusion granulation is 165°C, the temperature of the second stage is 180°C, the temperature of the third stage is 195°C, the temperature of the fourth stage is 165°C, and the temperature of the fifth stage is 140°C.

[0083] Table 1

[0084]

[0085] Performance Testing

[0086] According to GB / T1040, the tensile strength of the test composition samples 1-8, according to GB / T9341, the bending strength of the test composition samples 1-8, according to GB / T31402-2015, the antibacterial properties of the test composition samples 1-8. The following test results show that compared with ordinary bamboo fibers, the bamboo fibers modified with calcium carbonate can significantly improve the mechanical properties of polylactic acid degradable materials. In addition, zinc ions as antibacterial agents can improve the antibacterial and antimicrobial properties of polylactic acid degradable materials.

[0087] Table 2

[0088]

[0089] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A method for preparing a composition for a degradable cup cover, characterized in that: S100, feeding the lubricant, the compatibilizer, the toughening agent, the first polylactic acid and the second polylactic acid into a twin-screw extruder and mixing and stirring them uniformly according to the mass ratio of lubricant: compatibilizer: toughening agent: first polylactic acid: second polylactic acid = (1-2): (6-8): (6-8): (8-10): 100; S200, adding the glass fiber and the modified bamboo fiber to the twin-screw extruder at a mass ratio of glass fiber: modified bamboo fiber: second polylactic acid = (5-10): (15-20): 100 according to the amount of the second polylactic acid added in S100, mixing and stirring them evenly again, and extruding and granulating them together to obtain the composition for the degradable cup cover; The weight average molecular weight of the first polylactic acid is 5,000 to 10,000, and the weight average molecular weight of the second polylactic acid is 250,000 to 300,000; the modified bamboo fiber is surface-modified with calcium carbonate and loaded with an antibacterial agent.

2. The preparation method according to claim 1, characterized in that: The lubricant comprises at least one of fatty acid ester, fatty acid amide and polyethylene wax or a combination thereof; and / or The compatibilizer comprises at least one of maleic anhydride, methyl diphenyl diisocyanate, lysine triisocyanate, lysine diisocyanate, glycidyl methacrylate or a combination thereof; and / or The toughening agent comprises at least one of polybutylene succinate, polybutylene succinate adipate, polycaprolactone, polybutylene adipate terephthalate or a combination thereof; and / or The glass fiber includes at least one of silicate glass fiber, aluminosilicate glass fiber, alkali metal aluminosilicate glass fiber, alkaline earth metal aluminosilicate glass fiber, or a combination thereof.

3. The preparation method according to claim 1, characterized in that: The extrusion granulation temperature of the twin-screw extruder described in S200 is: first section: 160°C to 170°C, second section: 180°C to 190°C, third section: 190°C to 200°C, fourth section: 160°C to 170°C, and fifth section: 140°C to 150°C.

4. The preparation method according to any one of claims 1 to 3, characterized in that The antibacterial agent is an inorganic non-metallic oxide antibacterial agent.

5. The preparation method according to any one of claims 1 to 3, characterized in that: The preparation steps of the modified bamboo fiber include: S110, using a crusher to crush the bamboo fibers into bamboo fiber powder of target particle size; S120, soaking the bamboo fiber powder in hydrogen peroxide, adding an acetic acid aqueous solution of the same volume as the hydrogen peroxide after soaking and stirring simultaneously, leaving the mixture to stand after the addition is completed, filtering, washing, and drying the bamboo fiber powder; S130, uniformly dispersing the bamboo fiber powder obtained in S120 by ultrasonic dispersion in a calcium chloride aqueous solution, and dripping a sodium hydroxide aqueous solution until the pH reaches 11-12, to obtain a first mixture; S140, placing the first mixture in a closed reactor for aging, first evacuating the reactor, then introducing a gas including carbon dioxide into the reactor, stirring the first mixture under pressure to allow the first mixture to react with the carbon dioxide, stopping the introduction of the gas after the reaction is completed, releasing the pressure, extracting the solids, filtering, washing, and drying, to obtain the modified bamboo fiber.

6. The preparation method according to claim 5, characterized in that: The target particle size of the bamboo fiber powder in S110 is 400 mesh to 600 mesh; and / or The concentration of hydrogen peroxide in S120 is 20% to 25%; and / or The concentration of the acetic acid aqueous solution in S120 is 14% to 18%; and / or The soaking time in S120 is 2 hours to 3 hours, and the standing time is 20 minutes to 40 minutes; and / or The concentration of the calcium chloride aqueous solution in S130 is 10wt% to 20wt%; and / or The concentration of the sodium hydroxide aqueous solution in S130 is 8wt% to 12wt%; and / or The aging time in S140 is 12 to 18 hours; and / or The pressurization condition in S140 is 4 MPa to 8 MPa; and / or The stirring rate in S140 is 600 r / min to 800 r / min, and the stirring time is 2 h to 5 h.

7. The preparation method according to claim 5, characterized in that: After S140, the step of preparing the modified bamboo fiber further includes: S150, mixing the carboxymethyl cellulose and the starch in water, and placing the mixture in a water bath at 75° C. to 80° C. and stirring for 20 to 40 minutes to obtain gelatinized starch; S160, mixing maleic anhydride, ammonium persulfate, acrylic acid and acrylamide to obtain a second mixture; S170, lowering the temperature of the water bath to 50° C. to 60° C., adding the second mixture to the water bath according to the amount of starch in S150, and continuing to keep warm and stir for 1 h to 2 h to obtain modified starch; S180, mixing zinc chloride, the modified starch obtained in S170 and the modified bamboo fiber obtained in S140 in water, stirring evenly and letting stand for 4 to 6 hours, adding 8wt% to 12wt% sodium hydroxide aqueous solution until the pH reaches 11-12, letting stand again for 4 to 6 hours, filtering, washing and drying to obtain the bamboo fiber powder loaded with an antibacterial agent.

8. The preparation method according to claim 7, characterized in that: In S150, by mass ratio, carboxymethyl cellulose: starch: water = (2-4): (15-25): 100; and / or In S160, by mass ratio, maleic anhydride: ammonium persulfate: acrylic acid: acrylamide = (0.2-0.4): (1-1.5): (30-40): 100; and / or In S170, by mass ratio, the second mixture: starch = (10-20): 100; and / or In S180, by mass ratio, zinc chloride: modified starch: modified bamboo fiber: water = (6-8): (10-20): (20-30):

100.

9. A composition for a degradable cup cover, characterized in that: The composition for degradable cup covers is obtained by the preparation method according to any one of claims 1 to 8.

10. A cup cover, characterized in that: The cup cover is manufactured using the degradable cup cover composition obtained by the preparation method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Polylactic acid and plant fiber composite material and preparation method thereof

    CN101235192A

  • High-performance antibacterial long fiber-enhanced polylactic acid composite material and preparation method thereof

    CN104387734A

  • Biodegradable resin material and product thereof

    CN106589861A

  • High-temperature resistant polylactic acid composite material and molded product thereof

    CN107641302A

  • Preparation method and process of glass fiber / polylactic acid composite material

    CN111434716A