High-water-resistance bio-based degradable elastomer material and preparation method thereof
Through the melt blending process of bio-based colloidal copolymer and metal salt mixture, combined with modified acid soaking, the problem of poor water resistance of degradable elastomer materials is solved, and the combination of high water resistance and high elasticity is achieved, which improves the environmental protection of the material and sustainable application potential.
Patent Information
- Application Number
- CN202410873038.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-11-15
AI Technical Summary
The existing degradable elastomer materials have poor water resistance and are difficult to have high water resistance and high elasticity at the same time. Conventional modification methods damage the strength and biodegradability of the material, limiting their environmental protection and sustainable applications.
High water-resistant bio-based degradable elastomer materials composed of bio-based copolymers, metal salt mixtures and modified acids are prepared by melt blending and modified acid soaking processes to prepare high water-resistant elastomer without sacrificing degradability and strength. body material.
Without damaging the degradability and strength, the material's high elasticity and water resistance are achieved, which significantly improves the stability of the material in water, reduces the rate of absorption, and extends the service life.
Smart Images

Figure CN118956162A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of biodegradable materials, and in particular to a highly water-resistant bio-based degradable elastomer material and a preparation method thereof. Background Art
[0002] The extensive use of plastics has posed a serious threat to the global environment. Due to the long degradation cycle of plastics, it is difficult for them to be completely absorbed by the natural environment, which has led to a series of environmental problems such as marine pollution, soil pollution and ecological imbalance. Therefore, finding environmentally friendly materials to replace plastics has become an important task for global scientific researchers and industry.
[0003] In this context, degradable materials came into being. This material can be decomposed by biological and non-biological factors in the environment under certain conditions and converted into environmentally friendly substances such as carbon dioxide and water. This can not only reduce the impact on the environment, but also achieve sustainable utilization of resources. At present, degradable materials are mainly focused on the research and development of soft plastics and hard plastics, while there are relatively few studies on elastomers, which is undoubtedly an area worthy of attention and in-depth research.
[0004] Degradable elastomers are a special type of degradable material that combines the two properties of degradability and elasticity, and are therefore widely used in many fields, such as biomedicine, environmentally friendly packaging, agriculture, forestry, fishery, and marine engineering. However, despite these advantages of degradable elastomers, there is still significant room for improvement in their water resistance.
[0005] In many application scenarios, these materials are often exposed to water or humid environments. If their water resistance is poor, they may swell due to water absorption, change their shape and size, and degrade their performance, thus affecting their functions. At the same time, too high an absorption rate may cause the material to degrade faster in water, shortening its service life. Therefore, it is very important to optimize the water resistance of degradable elastomers.
[0006] Elastomers need to have good biodegradability and softness at the same time, which often requires the use of natural colloid materials. However, traditional biodegradable elastomers have poor tolerance to water and are prone to swelling and deformation, which to some extent limits the application and promotion of biodegradable elastomer materials.
[0007] In addition, most of the biodegradable elastomer materials are still in the laboratory research stage, and only a few have achieved large-scale production. This is mainly due to the cost limitations of raw materials and preparation processes, which make these materials difficult to be widely used in practice. Therefore, how to prepare biodegradable elastomer materials at low cost and high efficiency, and how to improve the water resistance of biodegradable elastomer materials, are key technical issues that need to be solved at present. Only by solving these problems can biodegradable elastomers truly realize their potential in environmental protection and sustainability, and provide an effective solution to the problem of plastic pollution. Summary of the invention
[0008] The present invention provides a highly water-resistant bio-based degradable elastomeric material and a preparation method thereof, aiming to solve the problems in the prior art that the bio-based degradable elastomeric material has poor water resistance, is easy to swell, is difficult to have both high water resistance and high elasticity, and conventional modification seriously damages the strength and biodegradability of the material. The prepared bio-based degradable elastomeric material has high elasticity and high water resistance without sacrificing degradability and strength.
[0009] The invention provides a highly water-resistant bio-based degradable elastomer material, the production raw materials of which include the following components in weight percentage: bio-based colloid copolymer (particles or powder), 20-50%; plasticizer (liquid), 1-30%; auxiliary agent (liquid), 1-30%; metal salt mixture, 1-50%; the raw materials are melt-blended at 60-120°C to obtain the bio-based degradable elastomer material.
[0010] Furthermore, the bio-based colloid copolymer is selected from one or more of xanthan gum, guar gum, gelatin, pectin and gum arabic.
[0011] Furthermore, the raw material composition of the metal salt mixture includes one or more of the following materials:
[0012] One or more metal salts formed by sodium as a cation combined with different acid radicals;
[0013] One or more metal salts formed by combining aluminum as a cation with different acid radicals;
[0014] One or more metal salts in which magnesium is used as a cation and is combined with different acid radicals;
[0015] The raw material composition of the metal salt is crushed, mixed and dried to obtain the powder of the metal salt mixture.
[0016] Furthermore, the water resistance of the bio-based degradable elastomer can be improved and can be preserved in water for more than 24 hours.
[0017] Furthermore, the ratio between the salts of each acid radical in the metal salt mixture is 1:(1.0-5.0) by mass if there are two salts, 1:(1.0-5.0) by mass if there are three salts, and 1:(1.0-5.0):(0.1-5.0) by mass if there are multiple salts. The ratio is 1:(1.0-5.0):(0.1-5.0):(0.1-5.0):…:(0.1-5.0):…:(0.1-5.0).
[0018] Furthermore, the plasticizer can be regarded as an edible plasticizer used in the food industry, preferably one or more of glycerol (glycerol), coconut oil, pectin, modified soybean lecithin and sorbitol, and more preferably glycerol (glycerol) or coconut oil.
[0019] Furthermore, the auxiliary agent may be an auxiliary agent conventionally used in the art, preferably one or more of a colorant, an antioxidant, and a moisture retainer:
[0020] The colorant is one or more of tomato red, lycopene, citrus yellow, sorghum red, riboflavin, black bean red, black currant red, safflower yellow, algae blue, etc.;
[0021] The antioxidant is one or more of D-isoascorbic acid, butylated hydroxyanisole (BHA), butylated hydroxytoluene (BHT), ascorbic acid (vitamin C), sorbic acid and its potassium salt, and disodium ethylenediaminetetraacetate;
[0022] The water retaining agent is one or more of propylene glycol, glycerol, polydextrose, calcium dihydrogen phosphate, potassium dihydrogen phosphate and maltitol.
[0023] The highly water-resistant bio-based degradable elastomer material is modified using a modified acid as a modifier, and the requirements for the modified acid and the modification are as follows:
[0024] (1) The modified acid is a monoprotic acid or a polyprotic acid, and the specific requirements are as follows:
[0025] a. The monoacid is an acid that can ionize an H + ion, such as hydrochloric acid, nitric acid, acetic acid, phenol, 3-indoleacetic acid, etc., one or more;
[0026] b. The polyacid is an acid that can ionize to produce two or more H+ ions, such as one or more of adipic acid, citric acid, succinic acid, tartaric acid, tannic acid and malic acid.
[0027] (2) The modification process comprises the following steps:
[0028] a. Weigh the raw material bio-based colloidal copolymer powder, plasticizer liquid and metal salt mixture according to weight percentage; heat the above materials in a water bath at 60-100° C. for 10-60 minutes, and then mix them evenly with one or more of the additives; continue heating and stirring for 2-50 minutes; the reaction is carried out in a melt blending device at a speed of 60-1000 rpm to obtain a highly water-resistant bio-based degradable elastomer material slurry; the slurry is injection molded and cooled at 0-10° C. to obtain a bio-based degradable elastomer material;
[0029] b. preparing a modified acid solution by mixing the modified acid with water, wherein the modified acid is one or more of a monoacid or a polyacid;
[0030] c. The bio-based degradable elastomeric material in step a is soaked in the modified acid solution prepared in step b and then taken out;
[0031] d. The highly water-resistant bio-based degradable elastomer material obtained in step c is rinsed with water and dried in sequence.
[0032] The present invention also provides a method for preparing the above-mentioned highly water-resistant bio-based degradable elastomer material, comprising the following steps:
[0033] (1) weighing raw materials bio-based colloidal copolymer powder, plasticizer liquid, and metal salt mixture according to weight percentage; wherein the bio-based colloidal copolymer is one or more of xanthan gum, guar gum, gelatin, pectin, and gum arabic; the plasticizer is one or more of glycerol (propylene glycol), coconut oil, etc.; the metal salt mixture is a raw material combination of metal salts, which is crushed, mixed, and dried to obtain a powder of the metal salt mixture;
[0034] (2) heating the material in a water bath at 60-100° C. for 10-60 min, and then mixing it evenly with one or more of the additives; continuing heating and stirring for 2-50 min;
[0035] (3) the reaction is carried out in a melt blending device at a rotation speed of 60-1000 rpm to obtain a highly water-resistant bio-based degradable elastomer material slurry; the slurry is injection molded and cooled at 0-10° C. to obtain a bio-based degradable elastomer material;
[0036] (4) preparing a modified acid solution by mixing the modified acid with water, wherein the modified acid is one or more of a monobasic acid or a polybasic acid;
[0037] (5) soaking the bio-based degradable elastomer material in step (3) in the modified acid solution prepared in advance in step (2) and then taking it out;
[0038] (6) The highly water-resistant bio-based degradable elastomer material obtained in step (5) is rinsed with water and dried in sequence.
[0039] Compared with the prior art, the advantages of the present invention are:
[0040] The bio-based degradable elastomer material has high elasticity and high water resistance without sacrificing degradability and strength. This solves the problems in the prior art that the bio-based degradable elastomer material has poor water resistance, is easy to swell, is difficult to have both high water resistance and high elasticity, and conventional modification seriously damages the strength and biodegradability of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Attached Figure 1 It is a comparison chart of the absorption rate of Examples 1-4 and the comparative example. DETAILED DESCRIPTION
[0042] The present invention is further described below in conjunction with examples, and the present invention can be better understood according to the following examples. However, the contents described in the examples are only used to illustrate the present invention, and these embodiments do not limit the present invention, and the changes in the reaction conditions, reactants or raw material amounts made by those of ordinary skill in the art according to these embodiments are all included in the protection scope of the present invention.
[0043] Comparative Example
[0044] (1) Weigh raw materials of bio-based colloidal copolymer powder and plasticizer liquid according to weight and volume (Table 1); wherein the bio-based colloidal copolymer is gelatin; the plasticizer is glycerol (propylene glycol); the metal salt mixture is sodium alginate; and the additives are propylene glycol, D-isoascorbic acid, lycopene and benzoic acid.
[0045] (2) heating the material in a water bath at 80°C for 15 min, then adding 30 mL of water; continuing heating and stirring for 2-50 min;
[0046] (3) The reaction is carried out in a melt blending device at a rotation speed of 250 rpm to obtain a highly water-resistant bio-based degradable elastomer material slurry; the slurry is injection molded and cooled at 4° C. to obtain a bio-based degradable elastomer material.
[0047] Table 1
[0048] Components specific ingredients Dosage Bio-based colloidal copolymers gelatin 21g Plasticizers glycerin 6mL Solvents water 20mL Metal salt mixture Sodium alginate 4.5g Additive 1 Propylene glycol 1mL Additive 2 D-isoascorbic acid 0.01g Additive 3 Tomato Red 0.024g Additive 4 benzoic acid 0.1g
[0049] (4) Prepare a modified acid solution by adding 10 g of tannic acid to 90 mL of water at 80° C. and stirring at 250 rpm in a stirring device to obtain a 10 wt % modified acid solution.
[0050] (5) soaking the bio-based degradable elastomer material in step (3) in the modified acid solution prepared in advance in step (4) and then taking it out;
[0051] (6) The highly water-resistant bio-based degradable elastomer material obtained in step (5) is rinsed with water and dried in sequence.
[0052] Example 1
[0053] (1) Weigh raw materials bio-based colloidal copolymer powder and plasticizer liquid according to weight and volume (Table 2); the bio-based colloidal copolymer is gelatin; the plasticizer is glycerol (propylene glycol); the metal salt mixture is sodium alginate, and the additives are propylene glycol, potassium sorbate, citrus yellow and benzoic acid.
[0054] (2) heating the raw materials (bio-based colloidal copolymer powder and plasticizer liquid) in a water bath at 80°C for 15 min, then adding 30 mL of water; continuing heating and stirring for 2-50 min;
[0055] (3) The reaction is carried out in a melt blending device at a rotation speed of 250 rpm to obtain a highly water-resistant bio-based degradable elastomer material slurry; the slurry is injection molded and cooled at 4° C. to obtain a bio-based degradable elastomer material.
[0056] Table 2
[0057]
[0058]
[0059] (4) Prepare a modified acid solution by adding 10 g of tannic acid to 90 mL of water at 80° C. and stirring at 250 rpm in a stirring device to obtain a 10 wt % modified acid solution.
[0060] (5) soaking the bio-based degradable elastomer material in step (3) in the modified acid solution prepared in advance in step (4) and then taking it out;
[0061] (6) The highly water-resistant bio-based degradable elastomer material obtained in step (5) is rinsed with water and dried in sequence.
[0062] Example 2
[0063] (1) Weigh raw materials bio-based colloidal copolymer powder and plasticizer liquid according to weight volume (Table 3); wherein the bio-based colloidal copolymer is gelatin; the plasticizer is glycerol (propylene glycol); the metal salt mixture is sodium alginate; and the additives are propylene glycol, disodium ethylenediaminetetraacetic acid, riboflavin and benzoic acid.
[0064] (2) heating the raw materials (bio-based colloidal copolymer powder and plasticizer liquid) in a water bath at 80°C for 15 min, then adding 30 mL of water; continuing heating and stirring for 2-50 min;
[0065] (3) The reaction is carried out in a melt blending device at a rotation speed of 250 rpm to obtain a highly water-resistant bio-based degradable elastomer material slurry; the slurry is injection molded and cooled at 4° C. to obtain a bio-based degradable elastomer material.
[0066] Table 3
[0067]
[0068]
[0069] (4) Prepare a modified acid solution by adding 20 g of tannic acid to 80 mL of water at 80° C. and stirring at 250 rpm in a stirring device to obtain a 10 wt % modified acid solution.
[0070] (5) soaking the bio-based degradable elastomer material in step (3) in the modified acid solution prepared in advance in step (4) and then taking it out;
[0071] (6) The highly water-resistant bio-based degradable elastomer material obtained in step (5) is rinsed with water and dried in sequence.
[0072] Example 3
[0073] (1) Weigh raw materials bio-based colloidal copolymer powder and plasticizer liquid according to weight volume (Table 4); the bio-based colloidal copolymer is gelatin; the plasticizer is glycerol (propylene glycol); the metal salt mixture is sodium alginate, and the additives are propylene glycol, butylated hydroxytoluene (BHT), black currant red and benzoic acid.
[0074] (2) heating the raw materials (bio-based colloidal copolymer powder and plasticizer liquid) in a water bath at 80°C for 15 min, then adding 30 mL of water; continuing heating and stirring for 2-50 min;
[0075] (3) The reaction is carried out in a melt blending device at a rotation speed of 250 rpm to obtain a highly water-resistant bio-based degradable elastomer material slurry; the slurry is injection molded and cooled at 4° C. to obtain a bio-based degradable elastomer material.
[0076] Table 4
[0077] Components specific ingredients Dosage Bio-based colloidal copolymers gelatin 21g Plasticizers glycerin 6mL Solvents water 20mL Metal salt mixture Sodium alginate 4.5g Additive 1 Propylene glycol 1mL Additive 2 Butylated Hydroxytoluene (BHT) 0.01g Additive 3 Blackcurrant red 0.024g Additive 4 benzoic acid 0.1g
[0078] (4) Prepare a modified acid solution by adding 30 g of tannic acid to 70 mL of water at 80° C. and stirring at 250 rpm in a stirring device to obtain a 10 wt % modified acid solution.
[0079] (5) soaking the bio-based degradable elastomer material in step (3) in the modified acid solution prepared in advance in step (4) and then taking it out;
[0080] (6) The highly water-resistant bio-based degradable elastomer material obtained in step (5) is rinsed with water and dried in sequence.
[0081] Example 4
[0082] (1) Weigh the raw material bio-based colloidal copolymer powder and plasticizer liquid according to weight volume (Table 5); the bio-based colloidal copolymer is gelatin; the plasticizer is glycerol (propylene glycol); the metal salt mixture is sodium alginate, and the additives are propylene glycol, butylated hydroxyanisole (BHA), phycocyanin and benzoic acid.
[0083] (2) heating the raw materials (bio-based colloidal copolymer powder and plasticizer liquid) in a water bath at 80°C for 15 min, then adding 30 mL of water; continuing heating and stirring for 2-50 min;
[0084] (3) The reaction is carried out in a melt blending device at a rotation speed of 250 rpm to obtain a highly water-resistant bio-based degradable elastomer material slurry; the slurry is injection molded and cooled at 4° C. to obtain a bio-based degradable elastomer material.
[0085] Table 5
[0086] Components specific ingredients Dosage Bio-based colloidal copolymers gelatin 21g Plasticizers glycerin 6mL Solvents water 20mL Metal salt mixture Sodium alginate 4.5g Additive 1 Propylene glycol 1mL Additive 2 Butylated Hydroxyanisole (BHA) 0.01g Additive 3 Algae blue 0.024g Additive 4 benzoic acid 0.1g
[0087] (4) Prepare a modified acid solution by adding 40 g of tannic acid to 60 mL of water at 80° C. and stirring at 250 rpm in a stirring device to obtain a 10 wt % modified acid solution.
[0088] (5) soaking the bio-based degradable elastomer material in step (3) in the modified acid solution prepared in advance in step (4) and then taking it out;
[0089] (6) The highly water-resistant bio-based degradable elastomer material obtained in step (5) is rinsed with water and dried in sequence.
[0090] The method for verifying the water resistance of a highly water-resistant bio-based degradable elastomer material of the present invention is as follows: the highly water-resistant bio-based degradable elastomer material prepared above is immersed in water for 24 hours and 48 hours, and the weight before immersion is recorded as Wd. It is particularly pointed out that the surface moisture of the material after immersion needs to be wiped off after it is taken out, and then the weight test is performed, and the weight is recorded as Ws. The weight of the material before and after immersion is calculated according to the following formula:
[0091] Q value swelling ratio (wt%) = (Ws-Wd) / Wd
[0092] The bio-based degradable elastomers prepared in Examples 1, 2, 3, 4 and the comparative example were selected to perform water resistance tests. The test results are shown in the attached figure. Figure 1 As shown, it can be seen that Examples 1-4 prepared by the present invention have obvious water resistance compared with the comparative example, among which the swelling rate of Example 3 after immersion for 48 hours is only 10.1%. Therefore, the present invention provides a highly water-resistant bio-based degradable elastomer material and a preparation method thereof, aiming to solve the problems in the prior art that the bio-based degradable elastomer material has poor water resistance, easy swelling, and is difficult to have the characteristics of high water resistance and high elasticity at the same time, and conventional modification seriously damages the strength and biodegradability of the material. The prepared bio-based degradable elastomer material has high elasticity and high water resistance without sacrificing degradability and strength.
[0093] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A highly water-resistant bio-based degradable elastomeric material, characterized in that: The production raw materials include the following components in weight percentage: Bio-based colloidal copolymers, 20-50%; Plasticizer, 1-30%; Metal salt mixture, 1-50%; Auxiliary agents, 1-30%; The raw materials are melt-blended at 60-120° C. to obtain the highly water-resistant bio-based degradable elastomer material.
2. The highly water-resistant bio-based degradable elastomeric material according to claim 1, characterized in that: The bio-based colloid copolymer is selected from one or more of xanthan gum, guar gum, gelatin, pectin and gum arabic.
3. The highly water-resistant bio-based degradable elastomeric material according to claim 1, characterized in that: The raw material composition of the metal salt mixture includes one or more of the following materials: One or more metal salts formed by sodium as a cation combined with different acid radicals; One or more metal salts formed by combining aluminum as a cation with different acid radicals; One or more metal salts in which magnesium is used as a cation and is combined with different acid radicals; The raw material composition of the metal salt is crushed, mixed and dried to obtain the powder of the metal salt mixture.
4. The highly water-resistant bio-based degradable elastomer material according to claim 3, characterized in that: The ratio between the salts of each acid radical in the metal salt mixture is 1:(1.0-5.0) by mass if there are two salts; 1:(1.0-5.0) by mass if there are three salts; and 1:(1.0-5.0) by mass if there are multiple salts; 1:(1.0-5.0) by mass:(0.1-5.0) by mass:(0.1-5.0) by mass:(0.1-5.0) by mass:(0.1-5.0) by mass:(0.1-5.0) by mass:(0.1-5.0) by mass:(0.1-5.0) by mass.
5. The highly water-resistant bio-based degradable elastomeric material according to claim 1, wherein: The plasticizer is selected from one or more of glycerol (propylene glycol), coconut oil, pectin, modified soybean lecithin and sorbitol.
6. The highly water-resistant bio-based degradable elastomeric material according to claim 1, characterized in that: The auxiliary agent is one or more of a colorant, an antioxidant, and a moisture retainer.
7. The highly water-resistant bio-based degradable elastomeric material according to claim 6, characterized in that: The colorant is one or more of tomato red, lycopene, citrus yellow, sorghum red, riboflavin, black bean red, black currant red, safflower yellow, and algae blue; The antioxidant is one or more of D-isoascorbic acid, butylated hydroxyanisole, butylated hydroxytoluene, ascorbic acid, sorbic acid and its potassium salt, and disodium ethylenediaminetetraacetate; The water retaining agent is one or more of propylene glycol, glycerol, polydextrose, calcium dihydrogen phosphate, potassium dihydrogen phosphate and maltitol.
8. The method for preparing a highly water-resistant bio-based degradable elastomer material according to any one of claims 1 to 7, characterized in that: The steps include: (1) weighing raw material bio-based colloidal copolymer powder, plasticizer liquid and metal salt mixture according to weight percentage; (2) heating the above materials in a water bath at 60-100° C. for 10-60 min, and then mixing them evenly with one or more of the additives; continuing heating and stirring for 2-50 min; (3) The reaction is carried out in a melt blending device at a rotation speed of 60-1000 rpm to obtain a highly water-resistant bio-based degradable elastomer material slurry; the slurry is injection molded and cooled at 0-10° C. to obtain a bio-based degradable elastomer material.
9. The method for preparing a highly water-resistant bio-based degradable elastomer material according to claim 8, characterized in that: The melt blending equipment is any one of an internal mixer, a single-screw extruder, an overhead stirrer or a twin-screw extruder; the cooling equipment is a cooling circulation pump with a constant temperature.
10. The method for modifying a highly water-resistant bio-based degradable elastomer material according to any one of claims 1 to 7, characterized in that: The bio-based degradable elastomer material is modified by using a modified acid as a modifier; The modified acid is a monoprotic acid or a polyprotic acid; The monoacid is a compound that can ionize to produce one H + Ionic acid, such as one or more of hydrochloric acid, nitric acid, acetic acid, phenol, 3-indoleacetic acid, etc.; The polyacid is capable of ionizing to generate 2 or more H + Ionic acids, such as one or more of adipic acid, citric acid, succinic acid, tartaric acid, tannic acid and malic acid; The modification process comprises the following steps: a. Weigh the raw material bio-based colloidal copolymer powder, plasticizer liquid and metal salt mixture according to weight percentage; heat the above materials in a water bath at 60-100° C. for 10-60 minutes, and then mix them evenly with one or more of the additives; continue heating and stirring for 2-50 minutes; the reaction is carried out in a melt blending device at a speed of 60-1000 rpm to obtain a highly water-resistant bio-based degradable elastomer material slurry; the slurry is injection molded and cooled at 0-10° C. to obtain a bio-based degradable elastomer material; b. preparing a modified acid solution with water, wherein the modified acid is one or more of a monoacid or a polyacid; c. The bio-based degradable elastomeric material in step a is soaked in the modified acid solution prepared in step b and then taken out; d. The highly water-resistant bio-based degradable elastomer material obtained in step c is rinsed with water and dried in sequence.