Photocuring self-repairing coating and preparation method thereof
By preparing a photocurable coating that combines uracil amino ketone groups and acrylate groups, the problem of paint film cracking during outdoor use was solved, achieving high mechanical strength and self-healing ability, and it is suitable for the field of photocurable coatings.
Patent Information
- Application Number
- CN202410809084.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-11-15
AI Technical Summary
Existing UV-cured coatings are prone to cracking and crazing when used outdoors, and their self-healing ability is insufficient.
A photocurable self-healing coating was prepared by synthesizing hydroxyl-terminated polyurethane, urea ester intermediate, and urethane intermediate, and combining uracil amino ketone groups with acrylate groups. The coating with self-healing function was formed by curing under a UV lamp.
It achieves rapid curing of the coating, good transparency, high mechanical strength and self-healing function at room temperature, making it suitable for outdoor use.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to a coating and a preparation method thereof, belonging to the technical field of photocuring coatings. Background Art
[0002] Photocuring technology is widely used in many fields due to its economy, high efficiency, energy saving, low carbon and environmental protection. Polyurethane acrylate is an important class of photocurable oligomers, which is characterized by its wide adaptability and is often used as a photocurable topcoat on the surface of substrates. In addition, polyurethane acrylate also has excellent chemical resistance, wear resistance and temperature resistance, making it often used as a coating on the surface of indoor objects. However, due to outdoor hot, humid and radiation environments, polyurethane acrylate coatings are prone to degradation and cracking, so how to design a self-repairing coating has become a topic of concern for many research teams. One of the methods is to enhance the heat resistance and mechanical strength of polyurethane acrylate by adding functional groups to the polymer chain segments.
[0003] In nature, the transmission of biological signals mainly relies on the interaction of non-covalent bonds. For example, the combination of two hydrogen bonds on adenine and thymine is essential for the replication and transcription of biological genetic information. However, for most polymers, the intermolecular hydrogen bond force is relatively small. To achieve the self-repair function, more polar functional groups need to be added to the molecular chain.
[0004] Therefore, there is an urgent need to propose a photocurable self-repairing coating and a preparation method thereof to solve the above technical problems. Summary of the invention
[0005] The purpose of the present invention is to provide a photocurable self-repairing coating and a preparation method thereof to solve the problems of cracking and crazing of the paint film of the current photocurable coating when used outdoors. A brief overview of the present invention is given below to provide a basic understanding of certain aspects of the present invention. It should be understood that this overview is not an exhaustive overview of the present invention. It is not intended to identify the key or important parts of the present invention, nor is it intended to limit the scope of the present invention.
[0006] The technical solution of the present invention:
[0007] A method for preparing a light-curable self-repairable coating comprises the following steps:
[0008] Synthesis of hydroxyl-terminated polyurethane;
[0009] Synthesis of urea ester intermediates;
[0010] Synthesis of urethane intermediates;
[0011] Synthesis of oligomers.
[0012] Preferably: the synthesis of hydroxyl-terminated polyurethane comprises the following steps:
[0013] Weigh a certain amount of glycidyl ether, dibasic acid and triphenyl phosphate into a three-necked flask, stir under the protection of nitrogen, and raise the temperature to 80°C-85°C. When a clear and transparent solution is formed in the flask, raise the temperature to 135°C-140°C, and react for 8h-9h to obtain a polyester product with hydroxyl groups at both ends;
[0014] The product was cooled to 45° C., a certain amount of isocyanate and dibutyltin dilaurate (DBTDL) were added, and the reaction was carried out for 6 h to 7 h to obtain a light yellow transparent hydroxyl-terminated polyurethane oligomer A.
[0015] Preferably: the synthesis of the urea ester intermediate comprises the following steps:
[0016] Under nitrogen conditions, 6-methylisocytosine was dissolved in a certain amount of toluene. After the dissolution was completed, a certain amount of isocyanate was added dropwise. The reaction temperature was 75° C., and a clear solution B was obtained after the reaction for 6 hours.
[0017] Preferably: in step 3, the synthesis of the urethane intermediate comprises the following steps:
[0018] Weigh a certain amount of ethyl acetate as solvent, add acrylate monomer and an appropriate amount of dibutyltin dilaurate (DBTDL) under nitrogen flow, add isocyanate dropwise after the temperature rises to 45°C-46°C, and react for 3h-3.5h after the addition is completed to obtain a transparent liquid C with isocyanate at one end and an acrylate double bond at the other end.
[0019] Preferably: A, B, and C are placed in a three-necked flask filled with nitrogen at a molar ratio of the active ingredients of 1:0-0.8:1.2-2, an appropriate amount of dibutyltin dilaurate (DBTDL) is added, the temperature is set to 45°C-46°C, the reaction time is 8h-8.5h, and an oligomer with an acrylate double bond at one end and a uracilamine group at the other end is obtained.
[0020] Preferably, the glycidyl ether is any one of allyl glycidyl ether, 2-biphenyl glycidyl ether, polyethylene glycol diglycidyl ether, tert-butyl glycidyl ether, glycidyl furfuryl ether, butyl glycidyl ether, C8-10 alkyl glycidyl ether, and polypropylene glycol diglycidyl ether, or a combination of at least two thereof.
[0021] Preferably, the dibasic acid is any one of sebacic acid, butynedioic acid, suberic acid, glutaconic acid, glutaric acid, malonic acid, azelaic acid, and pentadecanedioic acid, or a combination of at least two of them.
[0022] Preferably, the isocyanate is any one of p-phenylene diisocyanate, m-phenylenediisocyanate, 1,3-phenylene diisocyanate, toluene-2,4-diisocyanate, hexamethylene diisocyanate, L-lysine diisocyanate, and isophorone diisocyanate, or a combination of at least two thereof.
[0023] Preferably, the acrylic acid ester monomer is any one of hydroxyethyl acrylate, hydroxyethyl methacrylate, 2-(hydroxymethyl)methyl acrylate, 2-methyl-2-hydroxyethyl acrylate phosphate, 2-(hydroxymethyl)ethyl acrylate, and β-(m-hydroxyphenyl)hydroxyacrylic acid, or a combination of two thereof.
[0024] A light-curable self-repairing coating is prepared by the method, a certain amount of photoinitiator is added to the oligomer, the oligomer is evenly stirred and coated on a PET substrate, dried at room temperature overnight, and then cured under a UV lamp for 5-6 minutes to obtain the light-curable self-repairing coating.
[0025] The present invention has the following beneficial effects:
[0026] (1) Fast curing speed and high yield;
[0027] (2) Good paint film transparency;
[0028] (3) High mechanical strength;
[0029] (4) It can realize self-repair function at room temperature;
[0030] (5) The preparation method of the present invention is simple, easy to operate, low-cost and high-efficiency, and has great application value in the field of photocurable hard coating. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is described below by specific embodiments. However, it should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present invention. In addition, in the following description, the description of the known technology is omitted to avoid unnecessary confusion of the concept of the present invention.
[0032] Specific implementation method 1: A preparation method of a photocurable self-repairable coating of this implementation method, the present invention first synthesizes a polyester compound with terminal hydroxyl groups, and reacts it with isophorone diisocyanate (IPDI) to generate a polyurethane acrylate oligomer A with hydroxyl groups (-OH) at both ends; at the same time, 6-methylisocytosine is reacted with IPDI to obtain an intermediate compound B with a uracilamine ketone group at one end and an isocyanate at the other end; in addition, hydroxyethyl acrylate (HEA) is reacted with IPDI to obtain an intermediate compound C with an acrylate double bond at one end and an isocyanate at the other end; then, A, B, and C are stirred at a certain ratio and temperature, and a photocurable self-repairable polyurethane acrylate oligomer can be obtained after the reaction is completed; finally, 3wt% of a photoinitiator is added to the obtained product, and after irradiation with a 365nm mercury lamp for 5 minutes, a self-repairable UV coating can be obtained; the coating has good mechanical properties, good adhesion to plastic substrates, has a self-repairing function, is suitable for outdoor use, and has great application value in the field of photocurable coatings;
[0033] The following steps are involved:
[0034] Step 1: Synthesis of hydroxyl-terminated polyurethane;
[0035] Step 2: Synthesis of urea ester intermediate with self-repairing function;
[0036] Step 3: Synthesis of photosensitivity urethane intermediate;
[0037] Step 4: Synthesis of UV-curable self-healable oligomers.
[0038] Specific embodiment 2: In this embodiment, a method for preparing a photocurable self-repairing coating, the synthesis of hydroxyl-terminated polyurethane comprises the following steps:
[0039] Step 11: weigh glycidyl ether, dibasic acid and 0.5wt% triphenyl phosphate in a molar ratio of 2:1 and put them into a three-necked flask, stir under the protection of nitrogen, and raise the temperature to 80°C-85°C. When a clear and transparent solution is formed in the flask, raise the temperature to 135°C-140°C, and react for 8h-9h to obtain a polyester product with hydroxyl groups at both ends;
[0040] Step 12: Cool the obtained product to 45° C., add 0.1 mol of isocyanate and 0.2 wt % of dibutyltin dilaurate (DBTDL), and react for 6 h to 7 h to obtain a light yellow transparent hydroxyl-terminated polyurethane oligomer A.
[0041] Specific embodiment 3: In this embodiment, a method for preparing a photocurable self-repairing coating, the synthesis of a urea ester intermediate comprises the following steps:
[0042] Under nitrogen conditions, 6-methylisocytosine was dissolved in a certain amount of toluene. After the dissolution was completed, a certain amount of isocyanate was added dropwise. The mass ratio of 6-methylisocytosine to isocyanate was 1:8. The reaction temperature was 75°C. After reacting for 6 hours, a clear solution B whose main component was a urea intermediate was obtained.
[0043] Specific embodiment 4: In the preparation method of a light-curable self-repairable coating of this embodiment, in step 3, the synthesis of the urethane intermediate includes the following steps:
[0044] A certain amount of ethyl acetate was weighed as a solvent, and acrylate monomer and an appropriate amount of dibutyltin dilaurate (DBTDL) were added under nitrogen. After the temperature rose to 45°C-46°C, isocyanate was added dropwise, and the molar ratio of acrylate monomer to isocyanate was 1:1. After the addition was completed, the reaction was carried out for 3h-3.5h to obtain a transparent liquid C with isocyanate at one end and acrylate double bonds at the other end as the main component, which was an urethane intermediate.
[0045] Specific embodiment 5: A method for preparing a photocurable self-repairing coating in this embodiment, according to the molar ratio of terminal hydroxyl polyurethane oligomer, urea ester intermediate and urethane intermediate of 1:0-0.8:1.2-2, A, B, C are placed in a three-necked flask filled with nitrogen, 0.2wt% dibutyltin dilaurate (DBTDL) is added, the temperature is set to 45°C-46°C, the reaction time is 8h-8.5h, and an oligomer with an acrylate double bond at one end and a uracilamine ketone group at the other end is obtained; the present invention refers to a uracilamine ketone group recorded in Volume 4 of the journal Nature Structural Biology in 1997, pages 609-615, and the polymer with this group exhibits high physical cross-linking density and good self-repairing ability; through this example, the uracilamine ketone group is combined with the acrylate group to design a photocurable self-repairing coating.
[0046] Specific embodiment six: A method for preparing a photocurable self-repairable coating in this embodiment, wherein the glycidyl ether is any one of allyl glycidyl ether, 2-biphenyl glycidyl ether, polyethylene glycol diglycidyl ether, tert-butyl glycidyl ether, glycidyl furfural ether, butyl glycidyl ether, C8-10 alkyl glycidyl ether, and polypropylene glycol diglycidyl ether, or a combination of at least two of them, and the glycidyl ether is preferably butyl glycidyl ether.
[0047] Specific embodiment seven: This embodiment is a method for preparing a photocurable self-repairable coating, wherein the dibasic acid is any one of sebacic acid, butynedioic acid, suberic acid, glutaconic acid, glutaric acid, malonic acid, azelaic acid, and pentadecanedioic acid, or a combination of at least two of them, and the dibasic acid is preferably itaconic acid.
[0048] Specific embodiment eight: A method for preparing a photocurable self-repairable coating in this embodiment, wherein the isocyanate is any one of p-phenylene diisocyanate, m-phenylenediisocyanate, 1,3-phenylene diisocyanate, toluene-2,4-diisocyanate, hexamethylene diisocyanate, L-lysine diisocyanate, and isophorone diisocyanate, or a combination of at least two of them, and the isocyanate is preferably isophorone diisocyanate (IPDI).
[0049] Specific embodiment nine: A method for preparing a photocurable self-repairable coating in this embodiment, wherein the acrylate monomer is any one of hydroxyethyl acrylate, hydroxyethyl methacrylate, 2-(hydroxymethyl)methyl acrylate, 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate, 2-(hydroxymethyl)ethyl acrylate, and β-(m-hydroxyphenyl)hydroxyacrylate, or a combination of two of them, and the acrylate monomer is preferably hydroxyethyl acrylate.
[0050] Specific embodiment ten: A photocurable self-repairing coating in this embodiment is prepared by the method to obtain an oligomer, 2wt% of a photoinitiator is added to the oligomer, and the oligomer is coated on a PET substrate after sufficient stirring, dried at room temperature for 12h-16h, and cured under a UV lamp for 5-6 minutes to obtain a photocurable self-repairing coating; the improved UV coating (photocurable self-repairing coating) has the characteristics of high transparency, high mechanical strength, good adhesion and self-repairability.
[0051] Example 1
[0052] Resin Synthesis:
[0053] Synthesis of hydroxyl-terminated polyurethane A: Step 11: Weigh a certain amount of butyl glycidyl ether, itaconic acid and triphenyl phosphate into a three-necked flask, stir under the protection of nitrogen, and raise the temperature to 80°C; when a clear and transparent solution is formed in the flask, raise the temperature to 135°C, and react for 8 hours to obtain a polyester with hydroxyl groups at both ends;
[0054] Step 12: Cool the obtained product to 45° C., add a certain amount of IPDI and dibutyltin dilaurate (DBTDL), and react for 6 hours to obtain a light yellow transparent hydroxyl-terminated polyurethane oligomer;
[0055] Synthesis of photosensitive urethane intermediate C: Weigh a certain amount of ethyl acetate as solvent, add hydroxyethyl acrylate and an appropriate amount of DBTDL under nitrogen, add isocyanate dropwise after the temperature rises to 45°C, and react for 3 hours after the addition is completed to obtain a transparent liquid with an isocyanate end and an acrylate double bond at the other end;
[0056] Finally, A and C were placed in a three-necked flask filled with nitrogen at a molar ratio of 1:2, and an appropriate amount of DBTDL was added. The temperature was set to 45°C and the reaction time was 8 hours to obtain an oligomer with acrylate double bonds at both ends.
[0057] A certain amount of photoinitiator is added to the product, and the product is coated on a PET substrate after being fully stirred. After drying at room temperature overnight, the product is cured under a UV lamp for 5 minutes to obtain a light-cured self-repairing coating.
[0058] Performance characterization of light-cured repairable coating: Adhesion test: tested according to the Baige method, the substrate is PMMA; the test result is 5B; Mechanical properties: tested according to the national standard GB / T 16491-2008 biomaterial mechanical test method, the test results are: Young's modulus is 400MPa, and the breaking strength is 15MPa; The self-healing test result is: the paint film cannot be repaired at room temperature after breaking, and it cannot be repaired at 50°C.
[0059] Example 2
[0060] Resin Synthesis:
[0061] Synthesis of hydroxyl-terminated polyurethane A: Step 11: Weigh a certain amount of butyl glycidyl ether, itaconic acid and triphenyl phosphate into a three-necked flask, stir under the protection of nitrogen, and raise the temperature to 80°C; when a clear and transparent solution is formed in the flask, raise the temperature to 135°C, and react for 8 hours to obtain a polyester with hydroxyl groups at both ends;
[0062] Step 12: Cool the obtained product to 45° C., add a certain amount of IPDI and dibutyltin dilaurate (DBTDL), and react for 6 hours to obtain a light yellow transparent hydroxyl-terminated polyurethane oligomer;
[0063] Synthesis of self-repairable urea intermediate B: 6-methylisocytosine was dissolved in a certain amount of toluene under nitrogen conditions, and a certain amount of isocyanate was added dropwise after the dissolution was completed. The reaction temperature was 75°C, and a clear solution was obtained after the reaction for 6 hours.
[0064] Synthesis of photosensitive urethane intermediate C: Weigh a certain amount of ethyl acetate as solvent, add hydroxyethyl acrylate and an appropriate amount of DBTDL under nitrogen, add isocyanate dropwise after the temperature rises to 45°C, and react for 3 hours after the addition is completed to obtain a transparent liquid with an isocyanate end and an acrylate double bond at the other end;
[0065] Finally, A, B, and C were placed in a three-necked flask filled with nitrogen at an effective ingredient molar ratio of 1:0.2:1.8, and an appropriate amount of DBTDL was added. The temperature was set to 45°C and the reaction time was 8 h to obtain an oligomer with an acrylate double bond at one end and a uracilamine group at the other end.
[0066] A certain amount of photoinitiator is added to the product, and the product is coated on a PET substrate after being fully stirred. After drying at room temperature overnight, the product is cured under a UV lamp for 5 minutes to obtain a light-cured self-repairing coating.
[0067] Performance characterization of light-cured repairable coating: Adhesion test: According to the Baige method, the substrate is PMMA. The test result is 5B; Mechanical properties: The test is in accordance with the national standard GB / T 16491-2008 biomaterial mechanical test method, and the test results are: Young's modulus is 388MPa, and the fracture strength is 12.4MPa; The self-healing test result is: the paint film cannot be repaired at room temperature after breaking, and can be self-healed at 50℃ for 10 days.
[0068] Example 3
[0069] Resin Synthesis:
[0070] Synthesis of hydroxyl-terminated polyurethane A: Step 11: Weigh a certain amount of butyl glycidyl ether, itaconic acid and triphenyl phosphate into a three-necked flask, stir under the protection of nitrogen, and raise the temperature to 80°C; when a clear and transparent solution is formed in the flask, raise the temperature to 135°C, and react for 8 hours to obtain a polyester with hydroxyl groups at both ends;
[0071] Step 2: Cool the obtained product to 45° C., add a certain amount of IPDI and dibutyltin dilaurate (DBTDL), and react for 6 hours to obtain a light yellow transparent hydroxyl-terminated polyurethane oligomer;
[0072] Synthesis of self-repairable urea intermediate B: 6-methylisocytosine was dissolved in a certain amount of toluene under nitrogen conditions, and a certain amount of isocyanate was added dropwise after the dissolution was completed. The reaction temperature was 75°C, and a clear solution was obtained after the reaction for 6 hours.
[0073] Synthesis of photosensitive urethane intermediate C: Weigh a certain amount of ethyl acetate as solvent, add hydroxyethyl acrylate and an appropriate amount of DBTDL under nitrogen, add isocyanate dropwise after the temperature rises to 45°C, and react for 3 hours after the addition is completed to obtain a transparent liquid with an isocyanate end and an acrylate double bond at the other end;
[0074] Finally, A, B, and C were placed in a three-necked flask filled with nitrogen at an effective ingredient molar ratio of 1:0.4:1.6, and an appropriate amount of DBTDL was added. The temperature was set to 45°C and the reaction time was 8 h to obtain an oligomer with an acrylate double bond at one end and a uracilamine group at the other end.
[0075] A certain amount of photoinitiator is added to the product, and the product is coated on a PET substrate after being fully stirred. After drying at room temperature overnight, the product is cured under a UV lamp for 5 minutes to obtain a light-cured self-repairing coating.
[0076] Performance characterization of light-cured repairable coating: Adhesion test: According to the Baige method, the substrate is PMMA. The test result is 5B; Mechanical properties: According to the national standard GB / T 16491-2008 biomaterial mechanical test method, the test results are: Young's modulus is 380MPa, and the fracture strength is 11.7MPa; The self-healing test result is: the paint film can be repaired at room temperature for 15 days after breaking, and can be self-healed at 50℃ for 5 days.
[0077] Example 4
[0078] Resin Synthesis:
[0079] Synthesis of hydroxyl-terminated polyurethane A: Step 11: Weigh a certain amount of butyl glycidyl ether, itaconic acid and triphenyl phosphate into a three-necked flask, stir under the protection of nitrogen, and raise the temperature to 80°C; when a clear and transparent solution is formed in the flask, raise the temperature to 135°C, and react for 8 hours to obtain a polyester with hydroxyl groups at both ends;
[0080] Step 12: Cool the obtained product to 45° C., add a certain amount of IPDI and dibutyltin dilaurate (DBTDL), and react for 6 hours to obtain a light yellow transparent hydroxyl-terminated polyurethane oligomer;
[0081] Synthesis of self-repairable urea intermediate B: 6-methylisocytosine was dissolved in a certain amount of toluene under nitrogen conditions, and a certain amount of isocyanate was added dropwise after the dissolution was completed. The reaction temperature was 75°C, and a clear solution was obtained after the reaction for 6 hours.
[0082] Synthesis of photosensitive urethane intermediate C: Weigh a certain amount of ethyl acetate as solvent, add hydroxyethyl acrylate and an appropriate amount of DBTDL under nitrogen, add isocyanate dropwise after the temperature rises to 45°C, and react for 3 hours after the addition is completed to obtain a transparent liquid with an isocyanate end and an acrylate double bond at the other end;
[0083] Finally, A, B, and C were placed in a three-necked flask filled with nitrogen at an effective ingredient molar ratio of 1:0.6:1.4, and an appropriate amount of DBTDL was added. The temperature was set to 45°C and the reaction time was 8 h to obtain an oligomer with an acrylate double bond at one end and a uracilamine group at the other end.
[0084] A certain amount of photoinitiator was added to the product, and the product was coated on a PET substrate after being fully stirred. After drying at room temperature overnight, the product was cured under a UV lamp for 5 minutes to obtain a light-cured self-repairing coating.
[0085] Performance characterization of light-cured repairable coating: Adhesion test: According to the Baige method, the substrate is PMMA. The test result is 5B; Mechanical properties: According to the national standard GB / T 16491-2008 biomaterial mechanical test method, the test results are: Young's modulus is 375MPa, and the fracture strength is 11.1MPa; The self-healing test result is: the paint film can be repaired at room temperature for 13 days after breaking, and can be self-healed at 50℃ for 4 days.
[0086] Example 5
[0087] Resin Synthesis:
[0088] Synthesis of hydroxyl-terminated polyurethane A: Step 11: Weigh a certain amount of butyl glycidyl ether, itaconic acid and triphenyl phosphate into a three-necked flask, stir under the protection of nitrogen, and raise the temperature to 80°C; when a clear and transparent solution is formed in the flask, raise the temperature to 135°C, and react for 8 hours to obtain a polyester with hydroxyl groups at both ends;
[0089] Step 12: Cool the obtained product to 45° C., add a certain amount of IPDI and dibutyltin dilaurate (DBTDL), and react for 6 hours to obtain a light yellow transparent hydroxyl-terminated polyurethane oligomer;
[0090] Synthesis of self-repairable urea intermediate B: 6-methylisocytosine was dissolved in a certain amount of toluene under nitrogen conditions, and a certain amount of isocyanate was added dropwise after the dissolution was completed. The reaction temperature was 75°C, and a clear solution was obtained after the reaction for 6 hours.
[0091] Synthesis of photosensitive urethane intermediate C: Weigh a certain amount of ethyl acetate as solvent, add hydroxyethyl acrylate and an appropriate amount of DBTDL under nitrogen, add isocyanate dropwise after the temperature rises to 45°C, and react for 3 hours after the addition is completed to obtain a transparent liquid with an isocyanate end and an acrylate double bond at the other end;
[0092] Finally, A, B, and C were placed in a three-necked flask filled with nitrogen at an effective ingredient molar ratio of 1:0.8:1.2, and an appropriate amount of DBTDL was added. The temperature was set to 45°C and the reaction time was 8 h to obtain an oligomer with an acrylate double bond at one end and a uracilamine group at the other end.
[0093] A certain amount of photoinitiator is added to the product, and the product is coated on a PET substrate after being fully stirred. After drying at room temperature overnight, the product is cured under a UV lamp for 5 minutes to obtain a light-cured self-repairing coating.
[0094] Performance characterization of light-cured repairable coating: Adhesion test: According to the Baige method, the substrate is PMMA. The test result is 5B; Mechanical properties: The test is in accordance with the national standard GB / T 16491-2008 biomaterial mechanical test method, and the test results are: Young's modulus is 366MPa, and the fracture strength is 10.4MPa; The self-healing test result is: the paint film can be repaired at room temperature for 7 days after breaking, and can be self-healed at 50℃ for 1 day.
[0095] Example 6
[0096] Resin Synthesis:
[0097] Synthesis of hydroxyl-terminated polyurethane A: Step 11: Weigh a certain amount of butyl glycidyl ether, itaconic acid and triphenyl phosphate into a three-necked flask, stir under the protection of nitrogen, and raise the temperature to 80°C; when a clear and transparent solution is formed in the flask, raise the temperature to 135°C, and react for 8 hours to obtain a polyester with hydroxyl groups at both ends;
[0098] Step 12: Cool the obtained product to 45° C., add a certain amount of IPDI and dibutyltin dilaurate (DBTDL), and react for 6 hours to obtain a light yellow transparent hydroxyl-terminated polyurethane oligomer;
[0099] Synthesis of self-repairable urea intermediate B: 6-methylisocytosine was dissolved in a certain amount of toluene under nitrogen conditions, and a certain amount of isocyanate was added dropwise after the dissolution was completed. The reaction temperature was 75°C, and a clear solution was obtained after the reaction for 6 hours.
[0100] Synthesis of photosensitive urethane intermediate C: Weigh a certain amount of ethyl acetate as solvent, add hydroxyethyl acrylate and an appropriate amount of DBTDL under nitrogen, add isocyanate dropwise after the temperature rises to 45°C, and react for 3 hours after the addition is completed to obtain a transparent liquid with an isocyanate end and an acrylate double bond at the other end;
[0101] Finally, A, B, and C were placed in a three-necked flask filled with nitrogen at a molar ratio of 1:1:1, and an appropriate amount of DBTDL was added. The temperature was set to 45°C and the reaction time was 8 h to obtain an oligomer with an acrylate double bond at one end and a uracilamine group at the other end.
[0102] A certain amount of photoinitiator is added to the product, and the product is coated on a PET substrate after being fully stirred. After drying at room temperature overnight, the product is cured under a UV lamp for 5 minutes to obtain a light-cured self-repairing coating.
[0103] Performance characterization of light-cured repairable coating: Adhesion test: tested according to the Baige method, the substrate is PMMA; the test result is 5B; Mechanical properties: tested according to the national standard GB / T 16491-2008 biomaterial mechanical test method, the test results are: Young's modulus is 363MPa, and the breaking strength is 9.68MPa; Self-healing test results are: the paint film can be repaired at room temperature for 6 days after breaking, and can self-heal at 50°C for 12 hours.
[0104] Table 1 Summary of performance characteristics of the embodiments
[0105]
[0106] The embodiments described above are only descriptions of the preferred additive formula content of the present invention, and do not limit the overall concept and protection scope of the present invention. From the results, it can be seen that when other components remain unchanged, the greater the proportion of uracilamine in the polymer, the higher its self-healing efficiency, but the lower the overall Young's modulus and breaking strength of the paint film.
[0107] It should be noted that in the above embodiments, as long as the technical solutions are not contradictory, they can be arranged and combined, and those skilled in the art can exhaust all possibilities based on the mathematical knowledge of arrangement and combination. Therefore, the present invention will no longer describe the technical solutions after arrangement and combination one by one, but it should be understood that the technical solutions after arrangement and combination have been disclosed by the present invention.
[0108] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a light-curable self-repairing coating, characterized in that: The following steps are involved: Synthesis of hydroxyl-terminated polyurethane; Synthesis of urea ester intermediates; Synthesis of urethane intermediates; Synthesis of oligomers.
2. The method for preparing a light-curable self-repairable coating according to claim 1, characterized in that: The synthesis of hydroxyl-terminated polyurethane comprises the following steps: Weigh glycidyl ether, dibasic acid and triphenyl phosphate into a flask, stir under the protection of nitrogen, and raise the temperature to 80°C-85°C. When a clear and transparent solution is formed in the flask, raise the temperature to 135°C-140°C and react for 8h-9h to obtain a polyester product with hydroxyl groups at both ends; The product was cooled to 45° C., isocyanate and dibutyltin dilaurate were added, and the reaction was continued for 6 h to 7 h to obtain a light yellow transparent hydroxyl-terminated polyurethane oligomer A.
3. The method for preparing a light-curable self-repairable coating according to claim 1, characterized in that: The synthesis of the urea ester intermediate comprises the following steps: Under nitrogen conditions, 6-methylisocytosine was dissolved in toluene. After the dissolution was completed, isocyanate was added dropwise at 75°C. After reacting for 6 hours, a clear solution B was obtained.
4. The method for preparing a light-curable self-repairable coating according to claim 1, characterized in that: In step 3, the synthesis of the urethane intermediate comprises the following steps: Ethyl acetate was weighed as solvent, and acrylate monomer and dibutyltin dilaurate were added under nitrogen. After the temperature rose to 45°C-46°C, isocyanate was added dropwise and reacted for 3h-3.5h to obtain a transparent liquid C with an isocyanate end and an acrylate double bond at the other end.
5. A method for preparing a light-curable self-repairable coating according to any one of claims 1 to 4, characterized in that: A, B, and C are placed in a nitrogen-filled flask at an effective ingredient molar ratio of 1:0-0.8:1.2-2, dibutyltin dilaurate is added, the temperature is set to 45°C-46°C, the reaction time is 8h-8.5h, and an oligomer with an acrylate double bond at one end and a uracilamine group at the other end is obtained.
6. The method for preparing a light-curable self-repairable coating according to claim 2, characterized in that: The glycidyl ether is any one of allyl glycidyl ether, 2-biphenyl glycidyl ether, polyethylene glycol diglycidyl ether, tert-butyl glycidyl ether, glycidyl furfural ether, butyl glycidyl ether, C8-10 alkyl glycidyl ether, and polypropylene glycol diglycidyl ether, or a combination of at least two thereof.
7. The method for preparing a light-curable self-repairable coating according to claim 2, characterized in that: The dibasic acid is any one of sebacic acid, butynedioic acid, suberic acid, glutaconic acid, glutaric acid, malonic acid, azelaic acid, and pentadecanedioic acid, or a combination of at least two of them.
8. The method for preparing a light-curable self-repairable coating according to claim 3, characterized in that: The isocyanate is any one of p-phenylene diisocyanate, m-phenylenediisocyanate, 1,3-phenylene diisocyanate, toluene-2,4-diisocyanate, hexamethylene diisocyanate, L-lysine diisocyanate, and isophorone diisocyanate, or a combination of at least two thereof.
9. The method for preparing a light-curable self-repairable coating according to claim 4, characterized in that: The acrylic acid ester monomer is any one of hydroxyethyl acrylate, hydroxyethyl methacrylate, 2-(hydroxymethyl)methyl acrylate, 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate, 2-(hydroxymethyl)ethyl acrylate, and β-(m-hydroxyphenyl)hydroxyacrylic acid, or a combination of two thereof.
10. A light-curable self-repairable coating, characterized in that: An oligomer is prepared by the method according to any one of claims 1 to 9, a photoinitiator is added to the oligomer, the oligomer is coated on a substrate after stirring, dried at room temperature for 12 h to 14 h, and cured under a UV lamp for 5 to 6 minutes to obtain a light-cured self-repairing coating.
Citation Information
Patent Citations
Self-repairing polyurethane coating and preparation method thereof
CN104356338A
Bio-based photosensitive polyurethane resin, and self-repairing coating made of resin
CN105860017A
Preparing method of thermally-driven self-repairing elastomer based on hydrogen-bond interaction
CN106279619A
Disulfide bond and hydrogen bond-containing double self-repairing polyurethane coating for invisible car clothing and preparation method thereof