Vehicle-mounted encapsulating compound with good humidity and heat resistance and preparation method thereof

By preparing a combination of self-synthesized liquid crystal epoxy resin and self-synthesized linear phenolic resin, and combining benzene ring network crosslinking and liquid crystal ordered structure, the problems of poor adhesion and poor resistance to damp heat in the electronic control system of new energy vehicles were solved, and high-performance adhesion and electrical insulation effects were achieved.

CN118956307AActive Publication Date: 2024-11-15YANTAI DARBOND TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411098617.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-15
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

Existing encapsulating adhesives have problems such as poor adhesion, poor resistance to damp heat, poor resistance to high and low temperatures, and poor insulation performance in the electronic control systems of new energy vehicles, which cannot meet the performance requirements of intelligent and diversified development.

Method used

A combination of self-synthesized liquid crystal epoxy resin, self-synthesized linear phenolic resin, polyether-modified epoxy resin, and microencapsulated imidazole compounds was used to prepare a vehicle encapsulating adhesive with good resistance to damp heat through esterification and oxidation reactions. The combination of benzene ring network crosslinking and liquid crystal ordered structure improved the adhesion and electrical insulation properties.

Benefits of technology

The prepared encapsulating adhesive has good single-component workability, good adhesion, good flexibility, good resistance to damp heat, good resistance to high and low temperatures, and good electrical insulation properties, which meet the functional and reliability requirements of automotive module circuit boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to a vehicle-mounted encapsulating compound with good humidity and heat resistance. The vehicle-mounted encapsulating compound is prepared from the following raw materials: 10-25 parts of self-synthesized liquid crystal type epoxy resin, 15-35 parts of p-cresol formaldehyde epoxy resin, 10-15 parts of polyether modified epoxy resin, 32-37 parts of self-synthesized linear phenolic resin, 5-7 parts of a microcapsule type imidazole compound and 3-4 parts of fumed silica. The encapsulating compound prepared by the invention has the advantages of being good in single-component operability, good in adhesive property, good in flexibility, good in humidity and heat resistance, good in high and low temperature resistance, good in electrical insulation property and the like, and is suitable for sealing protection of circuit boards of various types of vehicle-mounted modules.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a vehicle-mounted encapsulation adhesive with good moisture and heat resistance, belonging to the field of adhesives. Background Art

[0002] With the advent of the era of intelligence, digitization, and diversification, the automotive industry has also ushered in new upgrades with the attributes of technology, consumption, and experience. New energy vehicles with new fields, new technologies, and new functions such as smart cockpits, smart driving, and smart clouds have become the main direction of future automotive industry development. As pure electric vehicles, new energy vehicles require the support of electronic control systems for vehicle control, motor control, and charging control. Electronic control systems play a vital role in the development of new energy vehicles. Encapsulation adhesives perform structural bonding and sealing protection on the integrated electronic components in the electronic control system of new energy vehicles. It has good process operability, high bonding performance, and good reliability, which effectively improves the functionality, stability, and safety of the electronic control system.

[0003] Most encapsulation adhesives have problems such as poor adhesion, poor moisture and heat resistance, poor high and low temperature resistance, and poor insulation performance. They cannot meet the various performance requirements brought about by the development of automotive electronic control system technology towards automation, intelligence, and diversification. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide an encapsulating glue with good moisture and heat resistance. The encapsulating glue prepared by the present invention has the advantages of good single-component operability, good bonding performance, good flexibility, good moisture and heat resistance, good high and low temperature resistance, and good electrical insulation performance.

[0005] The technical solution of the present invention to solve the above technical problems is as follows: a method for preparing a vehicle-mounted encapsulation adhesive with good moisture and heat resistance: a. By mass: add 13-14 parts of 4,4'-bis(2-hydroxyethoxy)biphenyl and 18-19 parts of N,N-dimethylformamide to the reactor, set the speed to 10RPM, and stir for 1-2h until completely dissolved; add 17-19 parts of 40% sodium hydroxide aqueous solution, heat to 85-95°C, set the speed to 10RPM, and vacuum stir for 1-2h; add 0.2-0.3 parts of benzyltriethylammonium chloride, dropwise add 49-51 parts of epichlorohydrin, complete within 30min, heat to 110-120°C, set the speed to 20RPM, condense and reflux and stir for 4-6h, and cool to room temperature; wash 2-3 times with a 3:1 mixed solution of anhydrous ethanol and acetone, dry at 60°C for 1-2h, and obtain a self-synthesized liquid crystal epoxy resin; b. By mass: 10-15 parts of resorcinol, 45-55 parts of 2,6-bis(hydroxymethyl)-p-cresol, and 35-40 parts of 40% formaldehyde aqueous solution are sequentially added into a reactor, the speed is set to 10 RPM under nitrogen protection, stirred for 0.5-1h, and mixed evenly; 0.3-0.5 parts of oxalic acid are added, heated to 55-65°C, the speed is set to 20RPM under nitrogen protection, stirred for 1-2h, and heated to 90-95°C; washed with deionized water 3-4 times, heated to 110-120°C, set the speed to 20RPM under vacuum conditions, and stirred for 2-3h to obtain a self-synthesized linear phenolic resin; c. By mass: 10 to 25 parts of self-synthesized liquid crystal epoxy resin, 15 to 35 parts of p-cresol epoxy resin, and 32 to 37 parts of self-synthesized linear phenolic resin are sequentially added into a stirring tank, heated to 45 to 55°C, set the speed to 30RPM, and stirred for 2 to 3 hours; cooled to room temperature, 10 to 15 parts of polyether-modified epoxy resin and 3 to 4 parts of fumed silica are sequentially added into a stirring tank, the speed is set to 30 RPM under vacuum conditions, and stirred for 1 to 2 hours, 5 to 7 parts of microcapsule-type imidazole compounds are added into a stirring tank, the speed is set to 20 RPM under vacuum conditions, and stirred for 2 to 3 hours to obtain an encapsulation glue.

[0006] The beneficial effects of the present invention are as follows: the encapsulation adhesive of the present invention has the characteristics of good single-component operability and good electrical insulation performance, which effectively meets the design and process diversity of vehicle-mounted module circuit board products. The good bonding performance is suitable for the structural bonding of various circuit board materials and related module electronic components, and has high applicability. The good flexibility, good moisture and heat resistance, and good high and low temperature resistance effectively ensure the functionality and reliability requirements of the vehicle-mounted module circuit board.

[0007] On the basis of the above technical solution, the present invention has also made the following improvements.

[0008] Furthermore, the synthesis mechanism of the self-synthesized liquid crystal epoxy resin is that the hydroxyl group in 4,4'-bis(2-hydroxyethoxy)biphenyl and the epoxy group in epichlorohydrin are synthesized into an epoxy compound having liquid crystal properties through esterification reaction and epoxidation reaction, and the specific reaction formula is as follows:

[0009] The beneficial effect of adopting the above further scheme is that the self-synthesized liquid crystal epoxy resin combines the advantages of liquid crystal order and benzene ring network cross-linking, and has good heat resistance, water resistance, and impact resistance; in addition, the liquid crystal epoxy resin also has the advantages of good resistance performance in the orientation direction, reducing free volume to improve flexibility and adhesion performance.

[0010] Furthermore, the o-cresol epoxy resin is SRN-1730 produced by Nanjing Yuelai New Material Technology Co., Ltd.

[0011] The beneficial effect of adopting the above further scheme is that the p-cresol-formaldehyde epoxy resin has excellent bonding strength and heat resistance, and also has excellent electrical insulation performance.

[0012] Furthermore, the synthesis mechanism of the self-synthesized linear phenolic resin is that the phenolic groups in resorcinol and 2,6-bis(hydroxymethyl)-p-cresol and the aldehyde groups in formaldehyde are oxidized under acidic conditions to synthesize the high-ortho linear phenolic resin, and the specific reaction formula is as follows:

[0013] The beneficial effect of adopting the above further scheme is that the structure of the ortho-methyl group and the para-methyl group of the benzene ring in the self-synthesized linear phenolic resin significantly improves the flexibility and regularity of the polymer molecular chain, and has good heat resistance, water resistance and adhesion properties. At the same time, the phenolic hydroxyl group on the molecular structure can be cured and cross-linked with the epoxy group under the promotion of tertiary amines, and has good reactivity and stability.

[0014] Furthermore, the polyether-modified epoxy resin is YLSE-2000 produced by Nanjing Yuelai New Material Technology Co., Ltd., and its specific structural formula is as follows:

[0015] The beneficial effect of adopting the above further scheme is that the polyether-modified epoxy resin introduces ether bonds into the epoxy resin molecular chain, so that it has the advantages of good flexibility, good bonding performance, good electrical insulation performance, etc.

[0016] Furthermore, the microcapsule-type imidazole compound is HX-3721 produced by Asahi Kasei Corporation of Japan.

[0017] The beneficial effect of adopting the above further scheme is that the microcapsule type imidazole compound adopts microencapsulation technology, uses liquid epoxy resin to wrap the imidazole component, and releases it when heated; it has the advantages of good stability, high reaction activity, and rapid curing at low temperature. DETAILED DESCRIPTION

[0018] The principles and features of the present invention are described below. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention. Example 1

[0019] a. By mass: 130 g of 4,4'-bis(2-hydroxyethoxy)biphenyl and 190 g of N,N-dimethylformamide were added to the reactor, the speed was set to 10 RPM, and the mixture was stirred for 1 h until completely dissolved; 170 g of 40% aqueous sodium hydroxide solution was added, the mixture was heated to 85°C, the speed was set to 10 RPM, and the mixture was stirred under vacuum for 2 h; 2 g of benzyltriethylammonium chloride was added, and 510 g of epichlorohydrin was added dropwise, and the mixture was completed within 30 min. The mixture was heated to 120°C, the speed was set to 20 RPM, the mixture was stirred under reflux for 6 h, and the mixture was cooled to room temperature; the mixture was washed twice with a mixed solution of anhydrous ethanol and acetone in a ratio of 3:1, and the mixture was dried at 60°C for 2 h to obtain a self-synthesized liquid crystal epoxy resin; b. By mass: 100 g of resorcinol, 550 g of 2,6-bis(hydroxymethyl)-p-cresol, and 350 g of 40% formaldehyde aqueous solution were sequentially added into a reactor, the speed was set to 10 RPM under nitrogen protection, stirred for 1 hour, and mixed evenly; 3 g of oxalic acid was added, heated to 55°C, the speed was set to 20 RPM under nitrogen protection, stirred for 2 hours, and heated to 95°C; washed with deionized water 3 times, heated to 120°C, the speed was set to 20 RPM under vacuum conditions, and stirred for 3 hours to obtain a self-synthesized linear phenolic resin; c. By mass: 200 g of self-synthesized liquid crystal epoxy resin, 250 g of para-cresol epoxy resin SRN-1730, and 350 g of self-synthesized linear phenolic resin were sequentially put into a stirring tank, heated to 50 ° C, set the speed to 30 RPM, and stirred for 2 h; cooled to room temperature, 100 g of polyether-modified epoxy resin YLSE-2000 and 40 g of fumed silica were sequentially put into a stirring tank, the speed was set to 30 RPM under vacuum conditions, and stirred for 2 h. 60 g of microcapsule-type imidazole compound HX-3721 was put into a stirring tank, the speed was set to 20 RPM under vacuum conditions, and stirred for 3 h to obtain an encapsulation glue. Example 2

[0020] a. By mass: 140 g of 4,4'-bis(2-hydroxyethoxy)biphenyl and 180 g of N,N-dimethylformamide were added to the reactor, the speed was set to 10 RPM, and the mixture was stirred for 1 h until completely dissolved; 190 g of 40% aqueous sodium hydroxide solution was added, the mixture was heated to 95°C, the speed was set to 10 RPM, and the mixture was stirred under vacuum for 0.5 h; 3 g of benzyltriethylammonium chloride was added, and 490 g of epichlorohydrin was added dropwise, and the mixture was completed within 30 min. The mixture was heated to 120°C, the speed was set to 20 RPM, the mixture was stirred under reflux for 4 h, and the mixture was cooled to room temperature; the mixture was washed twice with a mixed solution of anhydrous ethanol and acetone in a ratio of 3:1, and the mixture was dried at 60°C for 1 h to obtain a self-synthesized liquid crystal epoxy resin; b. By mass: 150 g of resorcinol, 450 g of 2,6-bis(hydroxymethyl)-p-cresol, and 400 g of 40% formaldehyde aqueous solution were sequentially added into a reactor, the speed was set to 10 RPM under nitrogen protection, stirred for 1 h, and mixed evenly; 5 g of oxalic acid was added, heated to 65 ° C, the speed was set to 20 RPM under nitrogen protection, stirred for 1 h, and heated to 90 ° C; washed with deionized water 4 times, heated to 110 ° C, set the speed to 20 RPM under vacuum conditions, and stirred for 2 h to obtain a self-synthesized linear phenolic resin; c. By mass: 100 g of self-synthesized liquid crystal epoxy resin, 350 g of para-cresol epoxy resin SRN-1730, and 320 g of self-synthesized linear phenolic resin were sequentially put into a stirring tank, heated to 50 ° C, set the speed to 30 RPM, and stirred for 3 h; cooled to room temperature, 150 g of polyether-modified epoxy resin YLSE-2000 and 30 g of fumed silica were sequentially put into a stirring tank, the speed was set to 30 RPM under vacuum conditions, and stirred for 1 h. 50 g of microcapsule-type imidazole compound HX-3721 was put into a stirring tank, the speed was set to 20 RPM under vacuum conditions, and stirred for 2 h to obtain an encapsulation glue. Example 3

[0021] a. By mass: 130 g of 4,4'-bis(2-hydroxyethoxy)biphenyl and 180 g of N,N-dimethylformamide were added to the reactor, the speed was set to 10 RPM, and the mixture was stirred for 1 h until completely dissolved; 190 g of 40% aqueous sodium hydroxide solution was added, the mixture was heated to 85°C, the speed was set to 10 RPM, and the mixture was stirred under vacuum for 1 h; 3 g of benzyltriethylammonium chloride was added, and 500 g of epichlorohydrin was added dropwise, and the mixture was completed within 30 min. The mixture was heated to 120°C, the speed was set to 20 RPM, the mixture was stirred under reflux for 5 h, and the mixture was cooled to room temperature; the mixture was washed 3 times with a mixed solution of anhydrous ethanol and acetone in a ratio of 3:1, and dried at 60°C for 2 h to obtain a self-synthesized liquid crystal epoxy resin; b. By mass: 120 g of resorcinol, 530 g of 2,6-bis(hydroxymethyl)-p-cresol, and 350 g of 40% formaldehyde aqueous solution were sequentially added into a reactor, the speed was set to 10 RPM under nitrogen protection, stirred for 1 h, and mixed evenly; 3 g of oxalic acid was added, heated to 65 ° C, the speed was set to 20 RPM under nitrogen protection, stirred for 2 h, and heated to 90 ° C; washed with deionized water 4 times, heated to 120 ° C, set the speed to 20 RPM under vacuum conditions, and stirred for 3 h to obtain a self-synthesized linear phenolic resin; c. By mass: 250 g of self-synthesized liquid crystal epoxy resin, 150 g of para-cresol epoxy resin SRN-1730, and 370 g of self-synthesized linear phenolic resin were sequentially put into a stirring tank, heated to 45 ° C, set the speed to 30 RPM, and stirred for 2 h; cooled to room temperature, 120 g of polyether-modified epoxy resin YLSE-2000 and 40 g of fumed silica were sequentially put into a stirring tank, the speed was set to 30 RPM under vacuum conditions, and stirred for 1 h. 70 g of microcapsule-type imidazole compound HX-3721 was put into a stirring tank, the speed was set to 20 RPM under vacuum conditions, and stirred for 3 h to obtain an encapsulation glue.

[0022] Comparative Example 1 a. By mass fraction: 100 g of resorcinol, 550 g of 2,6-bis(hydroxymethyl)-p-cresol, and 350 g of 40% formaldehyde aqueous solution were sequentially added into a reactor, the speed was set to 10 RPM under nitrogen protection, stirred for 1 hour, and mixed evenly; 3 g of oxalic acid was added, heated to 55°C, the speed was set to 20 RPM under nitrogen protection, stirred for 2 hours, and heated to 95°C; washed with deionized water 3 times, heated to 120°C, the speed was set to 20 RPM under vacuum conditions, and stirred for 3 hours to obtain a self-synthesized linear phenolic resin; b. By mass fraction: 200 g of bisphenol A solid epoxy resin, 250 g of para-cresol epoxy resin SRN-1730, and 350 g of self-synthesized linear phenolic resin were sequentially put into a stirring tank, heated to 50 ° C, set the speed to 30 RPM, and stirred for 2 h; cooled to room temperature, 100 g of polyether modified epoxy resin YLSE-2000 and 40 g of fumed silica were sequentially put into a stirring tank, the speed was set to 30 RPM under vacuum conditions, and stirred for 2 h. 60 g of microcapsule imidazole compound HX-3721 was put into a stirring tank, the speed was set to 20 RPM under vacuum conditions, and stirred for 3 h to obtain an encapsulation glue.

[0023] Comparative Example 2 a. By mass: 130 g of 4,4'-bis(2-hydroxyethoxy)biphenyl and 190 g of N,N-dimethylformamide were added to the reactor, the speed was set to 10 RPM, and the mixture was stirred for 1 h until completely dissolved; 170 g of 40% aqueous sodium hydroxide solution was added, the mixture was heated to 85°C, the speed was set to 10 RPM, and the mixture was stirred under vacuum for 2 h; 2 g of benzyltriethylammonium chloride was added, and 510 g of epichlorohydrin was added dropwise, and the mixture was completed within 30 min. The mixture was heated to 120°C, the speed was set to 20 RPM, the mixture was stirred under reflux for 6 h, and the mixture was cooled to room temperature; the mixture was washed twice with a mixed solution of anhydrous ethanol and acetone in a ratio of 3:1, and the mixture was dried at 60°C for 2 h to obtain a self-synthesized liquid crystal epoxy resin; b. By mass: 100 g of resorcinol, 550 g of 2,6-bis(hydroxymethyl)-p-cresol, and 350 g of 40% formaldehyde aqueous solution were sequentially added into a reactor, the speed was set to 10 RPM under nitrogen protection, stirred for 1 hour, and mixed evenly; 3 g of oxalic acid was added, heated to 55°C, the speed was set to 20 RPM under nitrogen protection, stirred for 2 hours, and heated to 95°C; washed with deionized water 3 times, heated to 120°C, the speed was set to 20 RPM under vacuum conditions, and stirred for 3 hours to obtain a self-synthesized linear phenolic resin; c. By mass: 200 g of self-synthesized liquid crystal epoxy resin, 250 g of bisphenol F epoxy resin, and 350 g of self-synthesized linear phenolic resin were sequentially put into a stirring tank, heated to 50 ° C, set the speed to 30 RPM, and stirred for 2 h; cooled to room temperature, 100 g of polyether-modified epoxy resin YLSE-2000 and 40 g of fumed silica were sequentially put into a stirring tank, the speed was set to 30 RPM under vacuum conditions, and stirred for 2 h. 60 g of microcapsule-type imidazole compound was put into a stirring tank, the speed was set to 20 RPM under vacuum conditions, and stirred for 3 h to obtain an encapsulation glue.

[0024] Comparative Example 3 a. By mass: 130 g of 4,4'-bis(2-hydroxyethoxy)biphenyl and 190 g of N,N-dimethylformamide were added to the reactor, the speed was set to 10 RPM, and the mixture was stirred for 1 h until completely dissolved; 170 g of 40% aqueous sodium hydroxide solution was added, the mixture was heated to 85°C, the speed was set to 10 RPM, and the mixture was stirred under vacuum for 2 h; 2 g of benzyltriethylammonium chloride was added, and 510 g of epichlorohydrin was added dropwise, and the mixture was completed within 30 min. The mixture was heated to 120°C, the speed was set to 20 RPM, the mixture was stirred under reflux for 6 h, and the mixture was cooled to room temperature; the mixture was washed twice with a mixed solution of anhydrous ethanol and acetone in a ratio of 3:1, and the mixture was dried at 60°C for 2 h to obtain a self-synthesized liquid crystal epoxy resin; b. By mass fraction: 250 g of self-synthesized liquid crystal epoxy resin and 350 g of para-cresol epoxy resin SRN-1730 were sequentially put into a stirring tank, heated to 50 ° C, set the speed to 30 RPM, and stirred for 2 h; cooled to room temperature, 150 g of polyether-modified epoxy resin YLSE-2000 and 40 g of fumed silica were sequentially put into a stirring tank, the speed was set to 30 RPM under vacuum conditions, and stirred for 2 h. 210 g of microencapsulated imidazole compound HX-3721 was put into a stirring tank, the speed was set to 20 RPM under vacuum conditions, and stirred for 3 h to obtain an encapsulation glue.

[0025] The performance of the edge sealing adhesives of the above-mentioned embodiments 1 to 3 of the present invention and comparative embodiments 1 to 3 was tested by the following tests. Among them, the single-component operability is characterized by the change rate of the encapsulating adhesive viscosity value, and the smaller the change rate, the better the operability; the bonding performance is characterized by the shear strength, and the larger the value, the better the bonding performance; the flexibility is characterized by the elongation at break, and the larger the value, the better the flexibility; the moisture and heat resistance is characterized by the change rate of the shear strength under high temperature and high humidity environment, and the smaller the change rate, the better the moisture and heat resistance; the high and low temperature resistance is characterized by the appearance of the adhesive layer of the sample after curing under high and low temperature alternating environment, and the absence of cracks in the appearance of the adhesive layer indicates good high and low temperature resistance; the electrical insulation performance is characterized by the value of the volume resistivity under high temperature and high humidity environment, and the larger the value, the better the electrical insulation performance.

[0026] Test Example 1 Operability Test Use Anton Paar viscometer, C35-2 rotor, 20 rpm, test the viscosity value at 25±1℃, and calculate the 8-hour rate of change in percentage (%).

[0027] Test Example 2 Adhesion Performance Test Use a universal testing machine, select FR4 Vs PCB material, and use the "Adhesive Tensile Shear Strength Test Method" at a temperature of 25°C and a shear rate of 10mm / min to test the shear strength before and after wet heat aging in megapascals (MPa); and calculate the attenuation rate before and after wet heat aging in percentage (%).

[0028] Test Example 3 Flexibility Test Use a universal testing machine to test the elongation at break in accordance with the "Test for Tensile Stress-Strain Properties of Vulcanized Rubber or Thermoplastic Rubber" in percentage (%).

[0029] Test Example 4 Moisture and heat resistance test Use a high temperature and high humidity environment box, set the temperature to 85℃ and the humidity to 85%RH, place the sample for 168 hours, then take it out and place it at room temperature for 4 hours; use a universal testing machine, select FR4 Vs PCB material, and use the "Adhesive Tensile Shear Strength Test Method" to test the shear strength at a temperature of 25℃ and a shear rate of 10mm / min. Calculate the change rate in percentage (%).

[0030] Test Example 5 High and Low Temperature Resistance Test Use a high and low temperature hot and cold shock box, set the conditions to -40 ~ 125 ° C, and after 500 cycles, observe whether the appearance of the sample glue layer is cracked.

[0031] Test Example 6 Electrical insulation performance test Use a high temperature and high humidity environment box, set the temperature to 85°C and the humidity to 85%. After placing the functional samples filled with encapsulation glue for 1000 hours, use an insulation resistance tester to test the volume resistivity of the functional samples after damp heat aging after powering on with a 5V DC power supply. The unit is ohm (Ω).

[0032] The test results are shown in Table 1 below.

[0033] Table 1 Test results of samples prepared in Examples 1 to 3 and Comparative Examples 1 to 3

[0034] From the data of shear strength and attenuation rate in Table 1, it can be seen that the combination of self-synthesized liquid crystal epoxy resin and self-synthesized linear phenolic resin has a significant gain effect on bonding performance and moisture and heat resistance, which is better than the use of either alone. From the data of volume resistivity in Table 1, it can be seen that the self-synthesized liquid crystal epoxy resin has a significant gain effect on electrical insulation performance. From the data of viscosity change rate in Table 1, it can be seen that the self-synthesized linear phenolic resin has a significant gain effect on operability. The encapsulating glue prepared by the present invention has the advantages of good single-component operability, good bonding performance, good flexibility, good moisture and heat resistance, good high and low temperature resistance, good electrical insulation performance, etc., and is suitable for circuit board sealing protection of various types of vehicle-mounted modules.

[0035] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A vehicle-mounted encapsulation adhesive with good moisture and heat resistance, characterized in that: The invention comprises, by weight, 10 to 25 parts of self-synthesized liquid crystal epoxy resin, 15 to 35 parts of p-cresol epoxy resin, 32 to 37 parts of self-synthesized linear phenolic resin, 10 to 15 parts of polyether modified epoxy resin, 3 to 4 parts of fumed silica and 5 to 7 parts of microcapsule type imidazole compound.

2. The vehicle-mounted encapsulation adhesive with good moisture and heat resistance according to claim 1, characterized in that: The self-synthesized liquid crystal epoxy resin is prepared from the following raw materials in parts by weight: 13 to 14 parts of 4,4'-bis(2-hydroxyethoxy)biphenyl, 18 to 19 parts of N,N-dimethylformamide, 17 to 19 parts of 40% sodium hydroxide aqueous solution, 0.2 to 0.3 parts of benzyltriethylammonium chloride, and 49 to 51 parts of epichlorohydrin.

3. The vehicle-mounted encapsulation adhesive with good moisture and heat resistance according to claim 2, characterized in that: The synthesis mechanism of the self-synthesized liquid crystal epoxy resin is that the hydroxyl group in 4,4'-bis(2-hydroxyethoxy)biphenyl and the epoxy group in epichlorohydrin are synthesized into a liquid crystal epoxy compound through esterification and epoxidation, and the specific structural formula is as follows: 。 4. The vehicle-mounted encapsulation adhesive with good moisture and heat resistance according to claim 2, characterized in that: The 4,4'-bis(2-hydroxyethoxy)biphenyl is a dihydroxybiphenyl compound with a molecular weight of 270-280 and a melting point of 190-200°C; the benzyltriethylammonium chloride is a triethylamine compound with a molecular weight of 220-230 and a melting point of 165-175°C.

5. The vehicle-mounted encapsulation adhesive with good moisture and heat resistance according to claim 1, characterized in that: The self-synthesized linear phenolic resin is prepared from the following raw materials in parts by weight: 10-15 parts of resorcinol, 45-55 parts of 2,6-bis(hydroxymethyl)-p-cresol, 35-40 parts of 40% formaldehyde aqueous solution, and 0.3-0.5 parts of oxalic acid.

6. The vehicle-mounted encapsulation adhesive with good moisture and heat resistance according to claim 5, characterized in that: The synthesis mechanism of the self-synthesized linear phenolic resin is that the phenolic groups in resorcinol and 2,6-bis(hydroxymethyl)-p-cresol and the aldehyde groups in formaldehyde are oxidized under acidic conditions to synthesize high-ortho linear phenolic resin, and its specific structural formula is as follows: 。 7. The vehicle-mounted encapsulation adhesive with good moisture and heat resistance according to claim 5, characterized in that: The resorcinol is a dihydroxybenzene substituted compound with a molecular weight of 100-110 and a melting point of 90-100°C; the 2,6-bis(hydroxymethyl)-p-cresol is a trihydroxy compound with a molecular weight of 170-180 and a melting point of 130-140°C.

8. The vehicle-mounted encapsulation adhesive with good moisture and heat resistance according to claim 1, characterized in that: The self-synthesized liquid crystal epoxy resin is a biphenyl liquid crystal epoxy resin with a softening point of 80 to 85°C and an epoxy equivalent of 190 to 200 g / eq; the p-ortho-cresol epoxy resin is a phenolic epoxy resin with a viscosity of 3000 to 5000 mPa·s at 25°C and an epoxy equivalent of 155 to 175 g / eq; the self-synthesized linear phenolic resin is a high-ortho-linear phenolic resin with a softening point of 80 to 85°C and a hydroxyl equivalent of 105-110 g / eq; the polyether-modified epoxy resin is a flexible epoxy resin with a viscosity of 1500 to 3000 mPa·s at 25°C and an epoxy equivalent of 240 to 260 g / eq; the microcapsule-type imidazole compound is an imidazole compound with a viscosity of 110,000 to 250,000 mPa·s at 25°C and a gel time of 11 to 13 min at 80°C.

9. According to claim 1, a vehicle-mounted encapsulation glue with good moisture and heat resistance, the preparation method of which is as follows: a. By mass: add 13-14 parts of 4,4'-bis(2-hydroxyethoxy)biphenyl and 18-19 parts of N,N-dimethylformamide to a reaction kettle, set the speed to 10RPM, and stir for 1-2 hours until completely dissolved; add 17-19 parts of 40% sodium hydroxide aqueous solution, heat to 85-95°C, set the speed to 10RPM, and vacuum stir for 1-2 hours; add 0.2-0.3 parts of benzyltriethylammonium chloride, drop 49-51 parts of epichlorohydrin, complete within 30 minutes, heat to 110-120°C, set the speed to 20RPM, condense reflux and stir for 4-6 hours, and cool to room temperature; wash 2-3 times with a 3:1 mixed solution of anhydrous ethanol and acetone, dry at 60°C for 1-2 hours to obtain a self-synthesized liquid crystal epoxy resin; b. By mass: 10-15 parts of resorcinol, 45-55 parts of 2,6-bis(hydroxymethyl)-p-cresol, and 35-40 parts of 40% formaldehyde aqueous solution are sequentially added into a reactor, the speed is set to 10 RPM under nitrogen protection, stirred for 0.5-1h, and mixed evenly; 0.3-0.5 parts of oxalic acid are added, heated to 55-65°C, the speed is set to 20RPM under nitrogen protection, stirred for 1-2h, and heated to 90-95°C; washed with deionized water 3-4 times, heated to 110-120°C, set the speed to 20RPM under vacuum conditions, and stirred for 2-3h to obtain a self-synthesized linear phenolic resin; c. By mass: 10 to 25 parts of self-synthesized liquid crystal epoxy resin, 15 to 35 parts of p-cresol epoxy resin, and 32 to 37 parts of self-synthesized linear phenolic resin are sequentially added into a stirring tank, heated to 45 to 55°C, set the speed to 30 RPM, and stirred for 2 to 3 hours; cooled to room temperature, 10 to 15 parts of polyether-modified epoxy resin and 3 to 4 parts of fumed silica are sequentially added into a stirring tank, the speed is set to 30 RPM under vacuum conditions, and stirred for 1 to 2 hours, 5 to 7 parts of microcapsule-type imidazole compounds are added into a stirring tank, the speed is set to 20 RPM under vacuum conditions, and stirred for 2 to 3 hours to obtain an encapsulation glue.

Citation Information

Patent Citations

  • Preparing methods of liquid crystal epoxy resin oligomer and epoxy resin composition

    CN101585821A

  • Preparation method of underfill adhesive with high electrical insulation property

    CN111394031A

  • Modified epoxy resin adhesive and preparation method thereof

    CN114410260A

  • Modified o-cresol formaldehyde epoxy resin and preparation method thereof

    CN115785394A

  • High thermal conductivity electrical insulation packaging material and preparation method therefor

    WO2021196510A1