Liquid reinforcing agent as well as preparation method and application thereof
The suspension stability and rheological performance of low-density cement slurry in deep-water surface cementing is improved through liquid reinforcement, which solves the problems of poor suspension stability and construction difficulties, and achieves efficient construction and low-cost demand for offshore cementing.
Patent Information
- Application Number
- CN202411014538.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
In deep-water surface cementing, low-density cement slurry has poor suspension stability and large usage. The existing methods have problems such as low slurry rate, complex formulation, high cost, and difficult construction, making it difficult to meet the needs of offshore cementing.
Provide a liquid reinforcement, including deionized water, alumina, silica, graphene oxide, inorganic suspension stabilizer, organic suspension stabilizer, tackifier and surfactant, and is prepared by reasonable proportioning and process treatment. A liquid reinforcement is produced to improve the early strength and rheological properties of low-density cement slurry.
It significantly improves the suspension stability and rheology performance of cement slurry, reduces the labor intensity of cementing operations, is suitable for offshore fully automatic liquid additive systems, realizes efficient cement hydration at low temperatures, has a wide temperature range, and the finished product can be used for a long time Stabilize storage.
Smart Images

Figure BDA0004965325030000141 
Figure BDA0004965325030000151
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cementing operations, and relates to a liquid enhancer and a preparation method and application thereof, and in particular to a liquid enhancer and a preparation method thereof for low-density cement slurry with a high water-cement ratio for offshore cementing. Background Art
[0002] Well cementing provides a solid guarantee for the development of offshore oil and gas resources, especially deepwater surface cementing. In deepwater surface cementing, due to the narrow pressure window, low-density cement slurry is usually used to balance the formation pressure, reduce the pressure difference between the cement slurry column and the formation pore pressure, and effectively prevent cement slurry leakage caused by low crushing pressure. Compared with land and shallow water surface cementing, the main challenges are:
[0003] (1) The deepwater surface pressure window is narrow, and low-density cement slurry is required for cementing. The suspension stability of low-density cement slurry has an important impact on the cementing quality, while the general low-density cement slurry system has poor suspension performance;
[0004] (2) Low-density cement slurry is used in deep-water surface cementing, which requires a lot of labor. When constructing the system, fewer types of admixtures and full liquidization are more suitable for on-site needs.
[0005] (3) The space on the offshore platform is small, and the number of cement ash tanks and slurry mixing equipment used is limited. The number of ash tanks is difficult to meet the requirements, and dust is easily generated on site, which is detrimental to the environment and the safety of workers. It is necessary to use low-density cement slurry with a high slurry making rate to facilitate on-site construction.
[0006] There are two main construction methods for low-density cement systems used in offshore cementing: low-density material reduction and high water-cement ratio reduction.
[0007] Low-density materials are mainly reduced by adding natural floating beads and artificial glass microspheres (<1g / cm 3 ) and other materials to achieve the effect of reducing the density of the system. Although the low-density cement slurry system constructed by this method has a fast strength development at low temperatures and can meet the needs of deep-water surface cementing operations, it has the following defects: low cement slurry production rate, complex formula composition; large amount of hollow microspheres, high operating costs, and not conducive to transportation and storage; limited on-site platform ash tanks, inconvenient material addition, and huge construction workload.
[0008] The reduction of high water-cement ratio is mainly achieved by adding water glass, soil, silica sol and other strong suspension materials to the cement slurry system to reduce the density of the system. The low-density cement slurry system constructed by this method has the advantages of simple formula, low operating cost and high slurry production rate, but there are problems such as slow strength development and difficult rheological adjustment during use.
[0009] Therefore, it is necessary to develop a liquid enhancer for low-density cement slurry systems with a high water-cement ratio. On the one hand, it can improve the early strength of the low-density cement slurry system. On the other hand, it can regulate the rheological properties of the cement slurry and improve the suspension stability of the cement slurry to meet the replacement requirements. Summary of the invention
[0010] In view of the defects of the prior art, the present invention provides a liquid enhancer and a preparation method and application thereof.
[0011] Specifically, the present invention provides a liquid enhancer, which includes, by weight: 100 parts of deionized water; 10 to 100 parts of aluminum oxide; 30 to 50 parts of silicon dioxide; 0.01 to 0.06 parts of graphene oxide; 1 to 3 parts of inorganic suspension stabilizer; 0.1 to 2 parts of organic suspension stabilizer; 2 to 6 parts of viscosity enhancer; and 0.1 to 1 part of surfactant.
[0012] The above-mentioned liquid enhancer, measured by weight, includes: 100 parts of deionized water; 10-80 parts of aluminum oxide; 35-50 parts of silicon dioxide; 0.01-0.05 parts of graphene oxide; 1-2.5 parts of inorganic suspension stabilizer; 0.1-1.5 parts of organic suspension stabilizer; 2.5-5.5 parts of viscosity enhancer; and 0.2-0.9 parts of surfactant.
[0013] The above-mentioned liquid enhancer, measured by weight, includes: 100 parts of deionized water; 20-60 parts of aluminum oxide; 40-50 parts of silicon dioxide; 0.02-0.04 parts of graphene oxide; 1-2 parts of inorganic suspension stabilizer; 0.5-1 part of organic suspension stabilizer; 3-5 parts of viscosity enhancer; and 0.3-0.7 parts of surfactant.
[0014] In the above-mentioned liquid reinforcing agent, the particle size of the aluminum oxide is 30nm to 200nm, and the particle size of the silicon dioxide is 10nm to 50nm.
[0015] The above-mentioned liquid enhancer, the inorganic suspension stabilizer includes one or more of nano bentonite, nano sepiolite, nano attapulgite and nano diatomaceous earth.
[0016] The above-mentioned liquid enhancer, the organic suspension stabilizer includes one or more of xanthan gum, guar gum, konjac gum and welan gum.
[0017] The above-mentioned liquid enhancer, the viscosity enhancer includes one or more of acrylic acid alkali swelling thickener ASE-60 or associative alkali swelling thickener TT935.
[0018] In the above-mentioned liquid enhancer, the surfactant is one or more of Tween-80, Triton X-100, polyethylene glycol, and hexadecyltrimethylammonium bromide.
[0019] In another aspect, the present invention provides a method for preparing the liquid enhancer, comprising:
[0020] (1) dissolving an inorganic suspension stabilizer and an organic suspension stabilizer in water and adjusting the pH to alkaline;
[0021] (2) adding a thickener solution and a surfactant solution and stirring;
[0022] (3) Add silicon dioxide, aluminum oxide, and graphene oxide and continue stirring;
[0023] (4) After aging for 1 to 2 hours, a liquid enhancer is obtained.
[0024] In the above-mentioned method for preparing the liquid enhancer, in steps (1) to (3), the pH of the mixed liquid is maintained at 8.5 to 9.5.
[0025] In another aspect, the present invention further provides the use of the liquid enhancer prepared by the above-mentioned preparation method in the preparation of a low-density cement slurry system with a high water-cement ratio for offshore cementing.
[0026] In the above application, the water-cement ratio of the cement slurry system is 0.66-1.96, and the density is 1.3-1.7 g / cm 3 .
[0027] The technical solution of the present invention has the following beneficial effects:
[0028] (1) The liquid enhancer of the present invention can effectively promote the cement hydration rate at low temperature, has obvious enhancement effect, can effectively control the rheological properties of the cement slurry system, improve the suspension stability of the system, and reduce free liquid;
[0029] (2) The liquid enhancer of the present invention is in liquid form, which is convenient for on-site construction and can be used in an offshore fully automatic liquid additive system, thereby reducing the labor intensity of cementing operations;
[0030] (3) The liquid enhancer of the present invention is in liquid form and has good compatibility with common cementing slurry systems. The prepared cement slurry has good rheological properties, no sedimentation, and a wide range of applications. It can be used at 20°C to 90°C for 1.3 to 1.7 g / cm 3 Cement slurry system;
[0031] (4) The liquid enhancer of the present invention can realize multifunctionality, and has the functions of low temperature enhancement, rheology adjustment, water loss control, stability improvement, etc., and is in liquid form, which meets the demand for offshore cementing liquid additives and is beneficial to offshore LAS construction;
[0032] (5) The liquid enhancer of the present invention is a new type of thickening suspension, and the preparation process temperature is room temperature and can be prepared under normal pressure without special process;
[0033] (6) The present invention successfully solves the compatibility problem between the thickening material and the ultrafine particle material, achieving the dual effects of thickening and improving strength. The final product is a liquid suspension that can be stably stored for a long time. DETAILED DESCRIPTION
[0034] In order to fully understand the purpose, features and effects of the present invention, the present invention is described in detail through the following specific embodiments. Except for the following contents, the process method of the present invention adopts conventional methods or devices in the art. Unless otherwise specified, the following terms have the meanings commonly understood by those skilled in the art.
[0035] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe a feature or characteristic, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0036] The liquid enhancer provided by the invention is a liquid enhancer for a low-density cement slurry system with a large water-cement ratio, and is composed of silicon dioxide, aluminum oxide, graphene oxide, an inorganic suspension stabilizer, an organic suspension stabilizer, a tackifier, and a surfactant.
[0037] Silica, alumina, and graphene oxide can work together. On the one hand, the stability of the suspension system can be improved by the close stacking and mutual support of the three. On the other hand, the three with different particle sizes can be filled into the pores of different pore sizes in the cement paste to improve the density of the cement paste and ultimately improve the compressive strength of the cement. Inorganic suspension stabilizers, organic suspension stabilizers, and thickeners stabilize the solid particles in the suspension system by increasing the viscosity of the liquid phase and increasing the shear force. At the same time, the temperature resistance of the three materials complements each other, effectively expanding the applicable temperature range of the suspension system. The three ultrafine powder materials of silica, alumina, and graphene oxide have a certain degree of hydrophobicity. The addition of surfactants can modify the surface of the three materials and increase their surface hydrophilicity, thereby increasing the content of solid particles in the suspension system.
[0038] The components of the liquid enhancer of the present invention are introduced in detail below.
[0039] Alumina
[0040] During the cement hydration process, the cement slurry becomes alkaline. The alumina in the enhancer dissolves into the pore solution in an alkaline environment, participates in the formation of monosulfide calcium sulfoaluminate hydrate (AFm) and enters into the calcium silicate hydrate (CSH) structure, thereby increasing the internal density of the cement paste and providing cement paste strength.
[0041] In some preferred embodiments, the particle size of the aluminum oxide is 30 nm to 200 nm. The present invention increases the solid content of the suspension system through particle grading by reasonably selecting the particle sizes of aluminum oxide and graphene oxide, and improves the suspension capacity of solid particles through close stacking and mutual support.
[0042] In some preferred embodiments, the weight percentage of aluminum oxide is 10 to 100 parts.
[0043] As an example, the weight percentage of aluminum oxide in the liquid enhancer of the present invention is 10 parts, 20 parts, 30 parts, 40 parts, 50 parts, 60 parts, 70 parts, 80 parts, 90 parts or 100 parts.
[0044] In practice, when the weight proportion of aluminum oxide is greater than 100 parts, the liquid enhancer will be severely thickened and the solution will lose fluidity.
[0045] In some more preferred embodiments, the weight percentage of aluminum oxide is 10 to 80 parts.
[0046] In some most preferred embodiments, the weight percentage of aluminum oxide is 20 to 60 parts.
[0047] Silicon dioxide
[0048] In liquid enhancers, silica can, on the one hand, fill the gaps between cement particles, provide nucleation sites for cement hydration, produce a filling effect, and thus increase the density of cement paste; on the other hand, silica has a certain volcanic ash effect, and can react with calcium hydroxide, a key element in cement hydration, to shorten the thickening time and improve the early strength.
[0049] In some preferred embodiments, the particle size of the silicon dioxide is 2 to 10 μm. If the particle size is too small, the solid content in the suspension system cannot be increased, and if the particle size is too large, the particles will settle and cannot be suspended for a long time.
[0050] In some preferred embodiments, the weight percentage of silicon dioxide is 30 to 50 parts.
[0051] As an example, the weight percentage of silicon dioxide in the liquid enhancer of the present invention is 30 parts, 35 parts, 40 parts, 45 parts or 50 parts.
[0052] In practice, when the weight proportion of silica is less than 30 parts, the reinforcing effect on cement paste will be weakened; when the weight proportion of silica is greater than 50 parts, it cannot be added to the solution because the solid content is too high.
[0053] In some more preferred embodiments, the weight percentage of silicon dioxide is 35 to 50 parts.
[0054] In some most preferred embodiments, the weight percentage of silicon dioxide is 40 to 50 parts.
[0055] Graphene oxide
[0056] Graphene oxide can enhance the mechanical properties of cement paste. When cement paste is damaged, damage is inevitable between the graphene oxide layers. The chemical bond breakage and interlayer peeling within the graphene oxide layer will consume energy, reduce the degree of damage to the cement paste, and thus improve the mechanical properties.
[0057] Wherein, the particle size of graphene oxide is 10nm to 50nm.
[0058] The present invention reasonably selects the particle sizes of aluminum oxide and graphene oxide, thereby increasing the solid content of the suspension system through particle grading on the one hand, and increasing the suspension capacity of solid particles through close stacking and mutual support on the other hand.
[0059] Among them, graphene oxide was purchased from Shanghai Naio Nano Technology Co., Ltd. with the product batch number NO-C-066-1.
[0060] In some preferred embodiments, the weight percentage of graphene oxide is 0.01 to 0.06 parts.
[0061] As an example, the weight percentage of graphene oxide in the liquid enhancer of the present invention is 0.01 parts, 0.02 parts, 0.03 parts, 0.04 parts, 0.05 parts or 0.06 parts.
[0062] In practice, when the weight proportion of graphene oxide is greater than 0.06 parts, it will bind a large amount of free water through surface wetting and adsorption, thereby reducing the fluidity of the cement slurry.
[0063] In some more preferred embodiments, the weight percentage of graphene oxide is 0.01 to 0.05 parts.
[0064] In some most preferred embodiments, the weight percentage of graphene oxide is 0.02 to 0.04 parts.
[0065] Inorganic suspension stabilizer
[0066] Inorganic suspension stabilizers are clay mineral materials that can be hydrated in the solution to form a network structure, increase the viscosity of the suspension, and play the role of suspending silica. At the same time, inorganic suspension stabilizers have good temperature resistance and can ensure the stability of the suspension under high temperature conditions.
[0067] In some preferred embodiments, the inorganic suspension stabilizer includes one or more of nano-bentonite, nano-sepiolite, nano-attapulgite, and nano-diatomaceous earth.
[0068] In some more preferred embodiments, the inorganic suspension stabilizer is nano-sepiolite.
[0069] In some preferred embodiments, the weight proportion of the inorganic suspension stabilizer is 1 to 3 parts.
[0070] As an example, the weight proportion of the inorganic suspension stabilizer in the liquid enhancer of the present invention is 1 part, 1.5 parts, 2 parts, 2.5 parts or 3 parts.
[0071] According to practice, when the weight proportion of the inorganic suspension stabilizer is less than 1 part, the silicon dioxide cannot be effectively suspended; when the weight proportion of the inorganic suspension stabilizer is greater than 3 parts, the suspension will cause gelation.
[0072] In some more preferred embodiments, the weight proportion of the inorganic suspension stabilizer is 1 to 2.5 parts.
[0073] In some most preferred embodiments, the weight portion of the inorganic suspension stabilizer is 1 to 2 parts.
[0074] Organic suspension stabilizer
[0075] Organic suspension stabilizers are made of bio-gum materials, which have the characteristics of small dosage, good viscosity-enhancing effect, good salt and temperature resistance, and can increase the shear force of the suspension and effectively suspend solid particles.
[0076] In some preferred embodiments, the organic suspension stabilizer includes one or more of xanthan gum, guar gum, konjac gum, and welan gum.
[0077] In some more preferred embodiments, the organic suspension stabilizer is xanthan gum.
[0078] In some preferred embodiments, the weight percentage of the organic suspension stabilizer is 0.1 to 2 parts.
[0079] As an example, the weight proportion of the organic suspension stabilizer in the liquid enhancer of the present invention is 0.1 parts, 0.5 parts, 1 parts, 1.5 parts or 2 parts.
[0080] In practice, when the weight proportion of the organic suspension stabilizer is less than 0.1 parts, the viscosity-enhancing effect is weak and the solid phase particles cannot be effectively suspended; when the weight proportion of the organic suspension stabilizer is greater than 2 parts, the suspension will be too thick and the solid phase material cannot be added.
[0081] In some more preferred embodiments, the weight percentage of the organic suspension stabilizer is 0.1 to 1.5 parts.
[0082] In some most preferred embodiments, the weight portion of the organic suspension stabilizer is 0.5 to 1 part.
[0083] Tackifier
[0084] The thickener material is an artificial synthetic polymer, which has good temperature and salt resistance. The addition of the thickener can enhance the suspension capacity of the solid phase material in the suspension, avoid sedimentation, and increase the upper temperature limit of the suspension system. On the other hand, it can increase the liquid phase viscosity of the cement slurry system and play a role in regulating the rheological properties of the cement slurry.
[0085] In some preferred embodiments, the tackifier includes one or more of acrylic acid alkali swelling thickener ASE-60 or associative alkali swelling thickener TT935.
[0086] Among them, acrylic acid alkali swelling thickener ASE-60 can be purchased from Shanghai Kain Chemical Co., Ltd.; associative alkali swelling thickener TT935 can be purchased from Guangzhou Runhong Chemical Co., Ltd.
[0087] The present invention selects an alkali swelling thickener as the thickener, which has a fast thickening time in an alkaline environment, good shear resistance, no stratification problem after thickening, high thickening efficiency and low dosage, and has good compatibility with the suspended material, thus solving the incompatibility between the thickening material and the ultrafine particles.
[0088] In some more preferred embodiments, the tackifier is acrylic alkali swelling thickener ASE-60.
[0089] In some preferred embodiments, the weight percentage of the tackifier is 2 to 6 parts.
[0090] As an example, the weight proportion of the viscosity enhancer in the liquid enhancer of the present invention is 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, 5.5 parts or 6 parts.
[0091] In practice, when the weight proportion of the thickener is less than 2 parts, a small amount of free liquid will appear in the enhancer suspension system, and the effect of improving the rheology of the cement slurry is weak; when the weight proportion of the thickener is greater than 6 parts, the viscosity of the suspension system is too high, and more solid phase materials cannot be added, resulting in a weakened reinforcement effect of the suspension.
[0092] In some more preferred embodiments, the weight percentage of the tackifier is 2.5 to 5.5 parts.
[0093] In some most preferred embodiments, the weight proportion of the tackifier is 3 to 5 parts.
[0094] Surfactants
[0095] The present invention improves the wetting and dispersibility of ultrafine particle materials by using a surfactant, can increase the solid content in the solution, improve the reinforcing effect on cement stone, and improve the dispersibility to avoid agglomeration and sedimentation of ultrafine materials.
[0096] In some preferred embodiments, the surfactant is one or more of Tween-80, Triton X-100, polyethylene glycol, and cetyltrimethylammonium bromide.
[0097] In some more preferred embodiments, the surfactant is Tween-80.
[0098] In some preferred embodiments, the weight portion of the surfactant is 0.1 to 1 part.
[0099] As an example, the weight percentage of the surfactant in the liquid enhancer of the present invention is 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part or 1 part.
[0100] In practice, when the weight proportion of the surfactant is less than 0.1 parts, some materials will not be modified, the wetting and dispersibility will be poor, agglomeration will easily occur, and more solid phase materials cannot be added; when the weight proportion of the surfactant is greater than 1 part, a large amount of foam will be generated when the suspension is stirred, and additional defoaming agent needs to be added for treatment.
[0101] In some more preferred embodiments, the weight portion of the surfactant is 0.2 to 0.9 parts.
[0102] In some most preferred embodiments, the weight portion of the surfactant is 0.3 to 0.7 parts.
[0103] On the other hand, the present invention also provides a method for preparing a liquid enhancer, comprising:
[0104] (1) dissolving a thickener in water to obtain a solution A;
[0105] (2) dissolving the surfactant in water to obtain solution B;
[0106] (3) dissolving an inorganic suspension stabilizer and an organic suspension stabilizer in water, and adjusting the pH to 8.5 to 9.5 using a 20% sodium hydroxide solution to obtain a solution C;
[0107] (4) Add solution C to the reactor, place in a water bath at room temperature and stir at a speed of 450-750 rpm, then add solution A and solution B, stir for 10 min until solutions A and B are evenly dispersed, then add silicon dioxide, aluminum oxide, and graphene oxide to the mixture, stir for 30 min, and maintain the pH of the mixture at 8.5-9.5.
[0108] (5) Aging the mixed solution prepared in the previous step for 1 to 2 hours to obtain a liquid enhancer.
[0109] In steps (1) to (3), the pH of the mixed solution is maintained at 8.5 to 9.5.
[0110] Among them, the ratio, composition and function of the components of silicon dioxide, aluminum oxide, graphene oxide, inorganic suspension stabilizer, organic suspension stabilizer, thickener, surfactant, etc. involved in the preparation method of the liquid enhancer of the present invention are the same as those of the liquid enhancer provided in the first aspect of the present invention, and the present invention will not repeat them here.
[0111] The preparation method of the liquid enhancer of the present invention is simple, the process temperature is room temperature, and it can be prepared under normal pressure. The liquid enhancer prepared according to the method of the present invention has good compatibility with common cementing slurry systems, and the prepared cement slurry has good rheological properties, no sedimentation, and a wide range of applications. It can be used for 1.3-1.7 g / cm at 20°C-90°C. 3 Cement slurry system. The present invention successfully solves the compatibility problem between the viscosity-enhancing material and the ultrafine particle material, achieving the dual effects of viscosity-enhancing and strength-enhancing, and the final product is a liquid suspension that can be stably stored for a long time.
[0112] Example
[0113] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions. The raw materials used in the following examples are all conventionally purchased.
[0114] Example 1
[0115] The liquid enhancer of this embodiment is composed of the following components in parts by weight: 100 parts of deionized water, 10 parts of aluminum oxide, 50 parts of silicon dioxide, 0.01 parts of graphene oxide, 1 part of nano-sepiolite, 0.1 parts of xanthan gum, 2 parts of acrylic acid alkali swelling thickener ASE-60, and 0.1 parts of surfactant Tween-80.
[0116] Wherein, the particle size of aluminum oxide is: 30nm~200nm;
[0117] The particle size of silicon dioxide is: 2 to 10 μm;
[0118] The particle size of graphene oxide is 10nm to 50nm.
[0119] The preparation method is:
[0120] (1) dissolving acrylic acid alkali swelling thickener ASE-60 in water to obtain solution A;
[0121] (2) dissolving the surfactant Tween-80 in water to obtain solution B;
[0122] (3) dissolving an inorganic suspension stabilizer, nano-sepiolite, and an organic suspension stabilizer, xanthan gum, in water, and adjusting the pH to 8.5 to 9.5 using a 20% sodium hydroxide solution to obtain a solution C;
[0123] (4) Add solution C to the reactor, place in a water bath at room temperature and stir at a speed of 450-750 rpm, then add solution A and solution B, stir for 10 min until solutions A and B are evenly dispersed, then add silicon dioxide, aluminum oxide, and graphene oxide to the mixture, stir for 30 min, and maintain the pH of the mixture at 8.5-9.5.
[0124] (5) Aging the mixed solution prepared in the previous step for 1 to 2 hours to obtain a liquid enhancer.
[0125] In steps (1) to (3), the pH of the mixed solution is maintained at 8.5 to 9.5.
[0126] Example 2
[0127] The liquid enhancer of this embodiment is composed of the following components in parts by weight: 100 parts of deionized water, 55 parts of aluminum oxide, 40 parts of silicon dioxide, 0.04 parts of graphene oxide, 2 parts of nano-sepiolite, 1 part of xanthan gum, 4 parts of acrylic acid alkali swelling thickener ASE-60, and 0.5 parts of surfactant Tween-80.
[0128] Wherein, the particle size of aluminum oxide is: 30nm~200nm;
[0129] The particle size of silicon dioxide is: 2 to 10 μm;
[0130] The particle size of graphene oxide is 10nm to 50nm.
[0131] The preparation method is:
[0132] (1) dissolving acrylic acid alkali swelling thickener ASE-60 in water to obtain solution A;
[0133] (2) dissolving the surfactant Tween-80 in water to obtain solution B;
[0134] (3) dissolving an inorganic suspension stabilizer, nano-sepiolite, and an organic suspension stabilizer, xanthan gum, in water, and adjusting the pH to 8.5 to 9.5 using a 20% sodium hydroxide solution to obtain a solution C;
[0135] (4) Add solution C to the reactor, place in a water bath at room temperature and stir at a speed of 450-750 rpm, then add solution A and solution B, stir for 10 min until solutions A and B are evenly dispersed, then add silicon dioxide, aluminum oxide, and graphene oxide to the mixture, stir for 30 min, and maintain the pH of the mixture at 8.5-9.5.
[0136] (5) Aging the mixed solution prepared in the previous step for 1 to 2 hours to obtain a liquid enhancer.
[0137] In steps (1) to (3), the pH of the mixed solution is maintained at 8.5 to 9.5.
[0138] Example 3
[0139] The liquid enhancer of this embodiment is composed of the following components in parts by weight: 100 parts of deionized water, 100 parts of aluminum oxide, 30 parts of silicon dioxide, 0.02 parts of graphene oxide, 3 parts of nano-sepiolite, 2 parts of xanthan gum, 6 parts of acrylic acid alkali swelling thickener ASE-60, and 1 part of surfactant Tween-80.
[0140] Wherein, the particle size of aluminum oxide is: 30nm~200nm;
[0141] The particle size of silicon dioxide is: 2 to 10 μm;
[0142] The particle size of graphene oxide is 10nm to 50nm.
[0143] The preparation method is:
[0144] (1) dissolving acrylic acid alkali swelling thickener ASE-60 in water to obtain solution A;
[0145] (2) dissolving the surfactant Tween-80 in water to obtain solution B;
[0146] (3) dissolving an inorganic suspension stabilizer, nano-sepiolite, and an organic suspension stabilizer, xanthan gum, in water, and adjusting the pH to 8.5 to 9.5 using a 20% sodium hydroxide solution to obtain a solution C;
[0147] (4) Add solution C to the reactor, place in a water bath at room temperature and stir at a speed of 450-750 rpm, then add solution A and solution B, stir for 10 min until solutions A and B are evenly dispersed, then add silicon dioxide, aluminum oxide, and graphene oxide to the mixture, stir for 30 min, and maintain the pH of the mixture at 8.5-9.5.
[0148] (5) Aging the mixed solution prepared in the previous step for 1 to 2 hours to obtain a liquid enhancer.
[0149] In steps (1) to (3), the pH of the mixed solution is maintained at 8.5 to 9.5.
[0150] Example 4
[0151] The liquid enhancer of this embodiment is composed of the following components in parts by weight: 100 parts of deionized water, 45 parts of aluminum oxide, 40 parts of silicon dioxide, 0.03 parts of graphene oxide, 1.5 parts of nano-sepiolite, 1 part of xanthan gum, 4 parts of acrylic acid alkali swelling thickener ASE-60, and 0.5 parts of surfactant Tween-80.
[0152] Wherein, the particle size of aluminum oxide is: 30nm~200nm;
[0153] The particle size of silicon dioxide is: 2 to 10 μm;
[0154] The particle size of graphene oxide is 10nm to 50nm.
[0155] The preparation method is:
[0156] (1) dissolving acrylic acid alkali swelling thickener ASE-60 in water to obtain solution A;
[0157] (2) dissolving the surfactant Tween-80 in water to obtain solution B;
[0158] (3) dissolving an inorganic suspension stabilizer, nano-sepiolite, and an organic suspension stabilizer, xanthan gum, in water, and adjusting the pH to 8.5 to 9.5 using a 20% sodium hydroxide solution to obtain a solution C;
[0159] (4) Add solution C to the reactor, place in a water bath at room temperature and stir at a speed of 450-750 rpm, then add solution A and solution B, stir for 10 min until solutions A and B are evenly dispersed, then add silicon dioxide, aluminum oxide, and graphene oxide to the mixture, stir for 30 min, and maintain the pH of the mixture at 8.5-9.5.
[0160] (5) Aging the mixed solution prepared in the previous step for 1 to 2 hours to obtain a liquid enhancer.
[0161] In steps (1) to (3), the pH of the mixed solution is maintained at 8.5 to 9.5.
[0162] Example 5
[0163] The liquid enhancer of this embodiment is composed of the following components in parts by weight: 100 parts of deionized water, 40 parts of aluminum oxide, 45 parts of silicon dioxide, 0.03 parts of graphene oxide, 1.5 parts of nano-sepiolite, 1 part of xanthan gum, 4 parts of acrylic acid alkali swelling thickener ASE-60, and 0.5 parts of surfactant Tween-80.
[0164] Wherein, the particle size of aluminum oxide is: 30nm~200nm;
[0165] The particle size of silicon dioxide is: 2 to 10 μm;
[0166] The particle size of graphene oxide is 10nm to 50nm.
[0167] The preparation method is:
[0168] (1) dissolving acrylic acid alkali swelling thickener ASE-60 in water to obtain solution A;
[0169] (2) dissolving the surfactant Tween-80 in water to obtain solution B;
[0170] (3) dissolving an inorganic suspension stabilizer, nano-sepiolite, and an organic suspension stabilizer, xanthan gum, in water, and adjusting the pH to 8.5 to 9.5 using a 20% sodium hydroxide solution to obtain a solution C;
[0171] (4) Add solution C to the reactor, place in a water bath at room temperature and stir at a speed of 450-750 rpm, then add solution A and solution B, stir for 10 min until solutions A and B are evenly dispersed, then add silicon dioxide, aluminum oxide, and graphene oxide to the mixture, stir for 30 min, and maintain the pH of the mixture at 8.5-9.5.
[0172] (5) Aging the mixed solution prepared in the previous step for 1 to 2 hours to obtain a liquid enhancer.
[0173] In steps (1) to (3), the pH of the mixed solution is maintained at 8.5 to 9.5.
[0174] Comparative Example
[0175] Comparative Examples 1-14 were prepared according to the same preparation method, wherein the raw materials in Comparative Examples 1-14 were the same as those in Example 1, and the raw material compositions of each comparative example were shown in Table 1. The preparation methods were as follows:
[0176] (1) dissolving acrylic acid alkali swelling thickener ASE-60 in water to obtain solution A;
[0177] (2) dissolving the surfactant Tween-80 in water to obtain solution B;
[0178] (3) dissolving an inorganic suspension stabilizer, nano-sepiolite, and an organic suspension stabilizer, xanthan gum, in water, and adjusting the pH to 8.5 to 9.5 using a 20% sodium hydroxide solution to obtain a solution C;
[0179] (4) Add solution C to the reactor, place in a water bath at room temperature and stir at a speed of 450-750 rpm, then add solution A and solution B, stir for 10 min until solutions A and B are evenly dispersed, then add silicon dioxide, aluminum oxide, and graphene oxide to the mixture, stir for 30 min, and maintain the pH of the mixture at 8.5-9.5;
[0180] (5) Aging the mixed solution prepared in the previous step for 1 to 2 hours to obtain a liquid enhancer.
[0181] In steps (1) to (3), the pH of the mixed solution is maintained at 8.5 to 9.5.
[0182] Table 1 Formulas used in Comparative Examples 1-14
[0183] formula Alumina Silicon dioxide Graphene oxide Nano sepiolite Xanthan gum ASE-60 Tween-80 Comparative Example 1 - 40 0.03 2 1 4 0.5 Comparative Example 2 60 - 0.03 2 1 4 0.5 Comparative Example 3 60 40 - 2 1 4 0.5 Comparative Example 4 - 40 - 2 1 4 0.5 Comparative Example 5 60 - - 2 1 4 0.5 Comparative Example 6 - - 0.06 2 1 4 0.5 Comparative Example 7 - - - 2 1 4 0.5 Comparative Example 8 40 45 0.03 - 1 4 0.5 Comparative Example 9 40 45 0.03 2 - 4 0.5 Comparative Example 10 40 45 0.03 2 1 - 0.5 Comparative Example 11 40 45 0.03 - - - 0.5 Comparative Example 12 40 45 0.03 - 1 - 0.5 Comparative Example 13 40 45 0.03 - - 4 0.5 Comparative Example 14 10 20 0.01 - - 2 -
[0184] Performance Testing
[0185] Liquid lightening cement slurry was prepared by using the liquid enhancers of the above embodiments and comparative examples. The formula of the liquid lightening cement slurry was as follows, in parts by weight: 100 parts of G-grade high sulfur resistant oil well cement, 0.5 parts of defoamer, 8 parts of fluid loss reducer, 6 parts of suspending agent, 5 parts of early strength agent, 1 part of retarder, 10 parts of the liquid enhancer prepared in Embodiments 1-5 or Comparative Examples 1-14, and 79 parts of artificial seawater. The cement slurry was prepared with reference to the oil well cement test method of GB / T19139-2012, and the rheological properties and compressive strength of the cement slurry were tested.
[0186] The G-grade high-sulfur-resistant oil well cement is produced by Shandong Zibo Zhongchang Special Cement Co., Ltd., and the defoaming agent C-DF60L, fluid loss reducer C-FL86L, suspending agent C-P81L, early strength agent C-A95L, and retarder C-R23L are all produced by Blue Ocean Boda Technology Co., Ltd.
[0187] The test performance results of the liquid lightening cement slurry prepared in Examples 1-5 and Comparative Examples 1-14 are as follows:
[0188] Table 2 Rheology and compressive strength of cement slurry formulations
[0189]
[0190]
[0191] Compared with Examples 1-5, the liquid enhancers prepared in Examples 1-7 do not add or add one or two of alumina, silica, and graphene oxide. The compressive strength of the cement slurry system constructed using the liquid enhancers of Examples 1-7 is significantly lower than that of the examples. This is because alumina, silica, and graphene oxide can fill the pores of cement stone, accelerate the cement hydration process, and thus improve the strength of cement stone. The liquid enhancers prepared in Examples 8-13 do not add or add one or two of nano sepiolite, xanthan gum, and ASE-60. The compressive strength of the cement slurry system constructed using the liquid enhancers of Examples 7-13 is close to that of Examples 1-5, with higher strength, but lower rheological properties than those of Examples 1-5. This is because nano sepiolite, xanthan gum, and ASE-60 can increase viscosity and shear force in the system, thereby regulating rheological properties. In Comparative Example 14, surfactant Tween-80 was added externally, and the solid phase components in the system could not be effectively dispersed, resulting in a low solid phase content of the liquid enhancer. Therefore, the rheological properties and compressive strength of the cement slurry prepared using Comparative Example 14 were relatively low.
[0192] The present invention has been disclosed above with preferred embodiments, but those skilled in the art should understand that these embodiments are only used to describe the present invention and should not be understood as limiting the scope of the present invention. It should be noted that all changes and substitutions equivalent to these embodiments should be deemed to be included in the scope of the claims of the present invention. Therefore, the scope of protection of the present invention should be based on the scope defined in the claims.
Claims
1. A liquid enhancer, characterized in that: The invention comprises, by weight: 100 parts of deionized water; 10 to 100 parts of aluminum oxide; 30 to 50 parts of silicon dioxide; 0.01 to 0.06 parts of graphene oxide; 1 to 3 parts of inorganic suspension stabilizer; 0.1 to 2 parts of organic suspension stabilizer; 2 to 6 parts of viscosity enhancer; and 0.1 to 1 part of surfactant.
2. The liquid enhancer according to claim 1, characterized in that The invention comprises, by weight: 100 parts of deionized water; 10 to 80 parts of aluminum oxide; 35 to 50 parts of silicon dioxide; 0.01 to 0.05 parts of graphene oxide; 1 to 2.5 parts of inorganic suspension stabilizer; 0.1 to 1.5 parts of organic suspension stabilizer; 2.5 to 5.5 parts of viscosity enhancer; and 0.2 to 0.9 parts of surfactant.
3. The liquid enhancer according to claim 1, characterized in that The invention comprises, by weight: 100 parts of deionized water; 20 to 60 parts of aluminum oxide; 40 to 50 parts of silicon dioxide; 0.02 to 0.04 parts of graphene oxide; 1 to 2 parts of inorganic suspension stabilizer; 0.5 to 1 part of organic suspension stabilizer; 3 to 5 parts of viscosity enhancer; and 0.3 to 0.7 parts of surfactant.
4. The liquid enhancer according to any one of claims 1 to 3, characterized in that The particle size of the aluminum oxide is 30 nm to 200 nm, and the particle size of the silicon dioxide is 10 nm to 50 nm.
5. The liquid enhancer according to any one of claims 1 to 3, characterized in that: The inorganic suspension stabilizer includes one or more of nano bentonite, nano sepiolite, nano attapulgite and nano diatomite.
6. The liquid enhancer according to any one of claims 1 to 3, characterized in that: The organic suspension stabilizer includes one or more of xanthan gum, guar gum, konjac gum and welan gum.
7. The liquid enhancer according to any one of claims 1 to 3, characterized in that The tackifier includes one or more of acrylic acid alkali swelling thickener ASE-60 or associative alkali swelling thickener TT935.
8. The liquid enhancer according to any one of claims 1 to 3, characterized in that The surfactant is one or more of Tween-80, Triton X-100, polyethylene glycol, and hexadecyltrimethylammonium bromide.
9. The method for preparing the liquid enhancer according to any one of claims 1 to 8, characterized in that: include: (1) dissolving an inorganic suspension stabilizer and an organic suspension stabilizer in water and adjusting the pH to alkaline; (2) adding a thickener solution and a surfactant solution and stirring; (3) Add silicon dioxide, aluminum oxide, and graphene oxide and continue stirring; (4) After aging for 1 to 2 hours, a liquid enhancer is obtained.
10. The method for preparing the liquid enhancer according to claim 9, characterized in that: In steps (1) to (3), the pH of the mixed solution is maintained at 8.5 to 9.
5.
11. Use of the liquid enhancer according to any one of claims 1 to 8 or the liquid enhancer prepared by the preparation method according to any one of claims 9 to 10 in preparing a low-density cement slurry system with a high water-cement ratio for offshore cementing.
12. The use according to claim 11, characterized in that: The water-cement ratio of the cement slurry system is 0.66-1.96, and the density is 1.3-1.7 g / cm 3 .