Semi-synthetic cutting fluid and preparation method thereof

By adding corrosion-resistant materials and foam-removing components to the cutting fluid, the existing cutting fluid has been solved, and the preparation of semi-synthetic cutting fluid with high efficiency, anti-corrosion, foam removal and long shelf life has been achieved, improving the mechanical equipment Anticorrosion performance and cutting fluid use effect.

CN118956472APending Publication Date: 2024-11-15DONGGUAN ESMAN LUBRICA TING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410933616.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing cutting fluid cannot effectively prevent corrosion of machinery and equipment when used, and it is easy to produce irritating odors and foam, affecting the use effect. It is difficult for super-strong additives to maintain the quality of the cutting fluid for a long time, resulting in deterioration.

Method used

Using the preparation method of semi-synthetic cutting fluid, by adding corrosion-resistant materials, defoaming components, deodorizing components and exogenous materials, including bubble-free aluminum corrosion inhibitor DX521, rapeseed oil, modified polydimethylsiloxane, iso- Thiazolinone, etc., combined with stirring and filtration steps, prepare cutting fluid with high corrosion resistance, foam removal effect and long shelf life.

Benefits of technology

It realizes efficient corrosion protection for mechanical equipment while ensuring lubrication, reduces corrosion, reduces environmental pollution, extends the shelf life of cutting fluid, improves processing accuracy and surface finish, and enhances the environmental protection characteristics and use effect of cutting fluid.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956472A_ABST
    Figure CN118956472A_ABST
Patent Text Reader

Abstract

The invention discloses a semi-synthetic cutting fluid and a preparation method thereof, and relates to the technical field of cutting fluid preparation, and the preparation method comprises the following steps: heating base oil to 75-85 DEG C, adding a corrosion-resistant material and a lubricant into the base oil while stirring, controlling the temperature of a first mixed solution at 60-75 DEG C, adding tall oil and triisopropanolamine into the first mixed solution, and stirring to obtain a second mixed solution; and mixing and stirring the first mixed solution and the second mixed solution for 20 minutes, adding an antibacterial agent, an antioxidant, a buffer agent and a stabilizer, adding an emulsifier, an extreme pressure agent and high-base-number synthetic calcium sulfonate into the composite solution, cooling, and filtering to obtain the semi-synthetic cutting fluid. According to the semi-synthetic cutting fluid and the preparation method thereof, friction between a tool and a workpiece is effectively reduced, abrasion is reduced, efficient corrosion prevention is achieved, foam generated by the cutting fluid is reduced, the using effect of the cutting fluid is improved, deterioration of the cutting fluid is delayed, temperature stability of the tool and the workpiece is maintained, and precision loss caused by overheating is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cutting fluid preparation, in particular to a semi-synthetic cutting fluid and a preparation method thereof. Background Art

[0002] Semi-synthetic metalworking fluid is an industrial liquid used in the process of metal cutting, chipping and grinding to cool and lubricate tools and workpieces. The cutting fluid is made of a variety of super-functional additives through scientific compound matching. It has good cooling performance, lubrication performance, rust prevention performance, oil removal and cleaning function, anti-corrosion function, and easy dilution. All indicators of cutting fluid are better than saponified oil. It has good cooling, cleaning, rust prevention and other characteristics.

[0003] Patent No. CN202210782364.4 discloses a cutting fluid and a preparation method thereof, wherein the cutting fluid includes a base oil balance by weight. The cutting fluid is a highly alkaline emulsified cutting fluid, which not only has a long service life, but also has a stable apparent state. The cutting fluid is not prone to turbidity, stratification and precipitation after standing, and the storage stability of the cutting fluid can meet the product use requirements. The cutting fluid does not contain toxic, harmful, environmentally polluting and irritating components such as borates and nitrites, and has better safety and environmental protection performance.

[0004] After searching the above patents, it was found that the cutting fluid has the following deficiencies: 1. Since the cutting fluid has good cooling performance, lubrication performance, rust prevention performance, oil removal and cleaning function, anti-corrosion function, and easy dilution characteristics, the cutting fluid cannot achieve efficient anti-corrosion for mechanical equipment while ensuring lubrication, which makes the surface of mechanical equipment that uses cutting fluid for cleaning and lubrication prone to corrosion problems; 2. When using the cutting fluid, it is not convenient to replace it in time, so that the cutting fluid will produce an irritating odor, affecting the use environment of the cutting fluid. At the same time, the cutting fluid contains foam, which will affect the use effect of the cutting fluid; 3. After the cutting fluid is used, the various super-strong additives inside make it difficult to ensure the quality of the cutting fluid for a long time, causing the cutting fluid to deteriorate easily.

[0005] Therefore, a semi-synthetic cutting fluid and a preparation method thereof are proposed to solve the above problems. Summary of the invention

[0006] The main purpose of the invention is to provide a method for preparing a semi-synthetic cutting fluid with strong anti-corrosion performance, good defoaming and deodorizing effects and long shelf life, which is applied to the preparation of the cutting fluid.

[0007] To achieve the above object, the technical solution adopted by the present invention is: a semi-synthetic cutting fluid and a preparation method thereof, comprising the following steps: Step 1: preparing a first mixed liquid, heating the base oil to 75°C to 85°C, adding the corrosion-resistant material and the lubricant to the base oil under stirring, and then stirring for 20min to 30min to obtain the first mixed liquid; Step 2: preparing a second mixed solution, controlling the temperature of the first mixed solution at 60° C. to 75° C., adding tall oil and triisopropanolamine to the first mixed solution, and adding a defoaming component and a deodorizing component, and then stirring for 20 min to 30 min to obtain a second mixed solution; Step 3: preparing a composite solution, mixing the first mixed solution and the second mixed solution for 20 minutes, adding an antimicrobial agent, an antioxidant, a buffer and a stabilizer, and then adding a shelf-life material, stirring for a second time for 20 minutes to obtain a composite solution; Step 4: Finished product, add emulsifier, extreme pressure agent and high base synthetic calcium sulfonate to the composite solution, then stir for 20min~30min, and control the temperature at 40℃~50℃, add polyacid triethanolamine ester for the second time, then stir for 20min~30min, control the temperature at 30℃~40℃ for the second time, add water, then stir for 20min~30min, stop heating and stir for 1.5h~2h, filter after cooling to obtain a semi-synthetic cutting fluid.

[0008] The corrosion-resistant material in step one includes bubbling aluminum corrosion inhibitor DX521, nitrite, triethanolamine and polymer synthetic fat. The weight ratio of each component of the corrosion-resistant material is 1%-5% of the bubbling aluminum corrosion inhibitor DX521 and 5%-10% of the polymer synthetic fat based on the total weight, which can effectively penetrate the foam film and destroy the foam structure.

[0009] The polymer synthetic fat includes rapeseed oil, and the weight ratio of the rapeseed oil is 1%-5% of the total weight. The polymer synthetic fat includes rapeseed oil, which has excellent biodegradability and low toxicity, and provides good environmental protection characteristics and lubricity for the cutting fluid.

[0010] The lubricant comprises one or more combinations of erucamide, graphite, molybdenum disulfide, fatty alcohol polyoxyethylene ether and nitrite; The weight ratio of each component of the lubricant is 2%-8% of erucamide, 2%-5% of graphite, 2%-15% of molybdenum disulfide, 5%-10% of fatty alcohol polyoxyethylene ether and 3%-7% of nitrite based on the total weight.

[0011] The defoaming component includes one or more of modified polydimethylsiloxane, polyether-modified silicone and nonylphenol polyoxyethylene ether.

[0012] The weight ratio of each component of the defoaming ingredient is 2%-8% of the total weight of modified polydimethylsiloxane, 3%-10% of polyether modified silicone and 5%-10% of nonylphenol polyoxyethylene ether. The modified polydimethylsiloxane helps the cutting fluid to better wet the metal surface and improve the spreading ability of the liquid, thereby improving the processing accuracy and surface finish. The polyether modified silicone can achieve defoaming and anti-foaming of the cutting fluid.

[0013] The deodorizing component comprises one or more of isothiazolinone, triazine compound, boric acid ester, polycarboxylic acid, heavy alkyl benzene sulfonate and tall oil amide.

[0014] The weight ratio of each component of the deodorizing ingredient is 3%-5% of isothiazolinone, 2%-5% of triazine compounds, 2%-3% of boric acid esters, 5%-10% of polycarboxylic acids, 5%-8% of heavy alkyl benzene sulfonates and 3%-5% of tall oil amide. Isothiazolinone, triazine compounds, boric acid esters, polycarboxylic acids, heavy alkyl benzene sulfonates and tall oil amide can deodorize the cutting fluid and reduce environmental pollution.

[0015] The antibacterial agent in step 3 is selected from at least one of triazines, isothiazolinones, morpholines or iodopropynyl butylcarbamate; The antioxidant is selected from at least one of triethanolamine, isopropanolamine or diglycolamine; The buffer is selected from at least one of sodium carbonate, sodium bicarbonate, acetic acid, citric acid or ammonia water.

[0016] The shelf life of the cutting fluid is prolonged and the deterioration of the cutting fluid can be delayed. In addition, the phenoxyethanol can ensure the uniformity of the cutting fluid and quickly take away the heat generated by friction.

[0017] The present invention has the following beneficial effects: 1. In the present invention, by adding corrosion-resistant materials and lubricants, non-foaming aluminum corrosion inhibitor DX521 and high molecular synthetic fat, the cutting fluid has low surface tension and high heat resistance, can effectively penetrate the foam film and destroy the foam structure, and the high molecular synthetic fat includes rapeseed oil, which has excellent biodegradability and low toxicity, and provides good environmental protection characteristics and lubricity for the cutting fluid. Nitrite effectively prevents the oxidation reaction of metals, and triethanolamine has good physical adsorption and lubricity, which can effectively reduce the friction between the tool and the workpiece, reduce wear, and make the cutting fluid more evenly distributed on the processing surface, thereby optimizing the cooling and cleaning process, so that while ensuring lubrication, it can achieve efficient corrosion protection for mechanical equipment and reduce corrosion of mechanical equipment.

[0018] 2. In the present invention, by adding defoaming components and deodorizing components, modified polydimethylsiloxane, polyether-modified silicone and nonylphenol polyoxyethylene ether, the modified polydimethylsiloxane helps the cutting fluid to better wet the metal surface and improve the spreading ability of the liquid, thereby improving the processing accuracy and surface finish. The polyether-modified silicone can achieve defoaming and foam suppression of the cutting fluid, and can increase the cooling effect of the cutting fluid, reduce the foam generated by the cutting fluid, and improve the use effect of the cutting fluid. Isothiazolinone, triazine compounds, boric acid esters, polycarboxylic acids, heavy alkyl benzene sulfonates and tall oil amide enable the cutting fluid to achieve deodorization and reduce environmental pollution.

[0019] 3. In the present invention, by adding a quality preservation material, the quality preservation material includes phenoxyethanol, which can extend the shelf life of the cutting fluid and delay the deterioration of the cutting fluid. Phenoxyethanol can also ensure the uniformity of the cutting fluid, quickly take away the heat generated by friction, help maintain the temperature stability of the tool and the workpiece, avoid the loss of precision caused by overheating, and increase the practicality of the cutting fluid. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The present invention is a schematic diagram of the overall process of a semi-synthetic cutting fluid and a preparation method thereof. DETAILED DESCRIPTION

[0021] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.

[0022] Comparative Example A semi-synthetic cutting fluid, the preparation method of the semi-synthetic cutting fluid comprises the following steps: Step 1: Prepare a first mixed liquid, heat the base oil to 75°C~85°C, and then stir for 20min~30min to obtain a first mixed liquid; Step 2: preparing a second mixed solution, controlling the temperature of the first mixed solution at 60° C. to 75° C., adding tall oil and triisopropanolamine to the first mixed solution, and then stirring for 20 min to 30 min to obtain a second mixed solution; Step 3: preparing a composite solution, mixing the first mixed solution and the second mixed solution for 20 minutes, adding an antibacterial agent, an antioxidant, a buffer and a stabilizer, and stirring for a second time for 20 minutes to obtain a composite solution; Step 4: Finished product, add emulsifier, extreme pressure agent and high base synthetic calcium sulfonate to the composite solution, then stir for 20min~30min, and control the temperature at 40℃~50℃, add polyacid triethanolamine ester for the second time, then stir for 20min~30min, control the temperature at 30℃~40℃ for the second time, add water, then stir for 20min~30min, stop heating and stir for 1.5h~2h, filter after cooling to obtain a semi-synthetic cutting fluid.

[0023] The comparative example is a preparation step of preparing a semi-finished cutting fluid in the prior art. The comparative example is compared with Example 1, Example 2 and Example 3, and the comparison results are as follows.

[0024] Embodiment 1 Please refer to Figure 1 As shown: A semi-synthetic cutting fluid and a preparation method thereof, comprising the following steps: Step 1: preparing a first mixed liquid, heating the base oil to 75°C-85°C, adding corrosion-resistant materials including a foam-free aluminum corrosion inhibitor DX521, nitrite, triethanolamine and a polymer synthetic fat and a lubricant including erucamide, graphite, molybdenum disulfide, fatty alcohol polyoxyethylene ether and nitrite to the base oil under stirring, and then stirring for 20min-30min to obtain a first mixed liquid; Step 2: preparing a second mixed solution, controlling the temperature of the first mixed solution at 60° C. to 75° C., adding tall oil and triisopropanolamine to the first mixed solution, and then stirring for 20 min to 30 min to obtain a second mixed solution; Step 3: preparing a composite solution, mixing the first mixed solution and the second mixed solution for 20 minutes, adding an antibacterial agent, an antioxidant, a buffer and a stabilizer, and stirring for a second time for 20 minutes to obtain a composite solution; Step 4: Finished product, add emulsifier, extreme pressure agent and high base synthetic calcium sulfonate to the composite solution, then stir for 20min~30min, and control the temperature at 40℃~50℃, add polyacid triethanolamine ester for the second time, then stir for 20min~30min, control the temperature at 30℃~40℃ for the second time, add water, then stir for 20min~30min, stop heating and stir for 1.5h~2h, filter after cooling to obtain a semi-synthetic cutting fluid.

[0025] The corrosion-resistant material in step one includes bubbling-free aluminum corrosion inhibitor DX521, nitrite, triethanolamine and polymer synthetic fat. The weight ratio of each component of the corrosion-resistant material is 1%-5% of the bubbling-free aluminum corrosion inhibitor DX521 and 5%-10% of the polymer synthetic fat based on the total weight.

[0026] The high molecular weight synthetic fat includes rapeseed oil, and the weight proportion of the rapeseed oil is 1%-5% of the total weight.

[0027] The lubricant includes one or more combinations of erucamide, graphite, molybdenum disulfide, fatty alcohol polyoxyethylene ether and nitrite; The weight ratio of each component of the lubricant is 2%-8% of erucamide, 2%-5% of graphite, 2%-15% of molybdenum disulfide, 5%-10% of fatty alcohol polyoxyethylene ether and 3%-7% of nitrite based on the total weight.

[0028] Through the above-mentioned proportions, the cutting fluid prepared in Example 1 and the comparative example has the following advantages: it can effectively penetrate the foam film and destroy the foam structure; at the same time, the polymer synthetic ester includes rapeseed oil, which has excellent biodegradability and low toxicity, and provides good environmental protection characteristics and lubricity for the cutting fluid; nitrite effectively prevents the oxidation reaction of metals; triethanolamine has good physical adsorption and lubricity, and can effectively reduce the friction between the tool and the workpiece, reduce wear, and make the cutting fluid more evenly distributed on the processing surface, thereby optimizing the cooling and cleaning process, so that while ensuring lubrication, it can achieve efficient corrosion protection for mechanical equipment and reduce corrosion of mechanical equipment.

[0029] Embodiment 2 Please refer to Figure 1 As shown: A semi-synthetic cutting fluid and a preparation method thereof, comprising the following steps: Step 1: Prepare a first mixed liquid, heat the base oil to 75°C~85°C, and then stir for 20min~30min to obtain a first mixed liquid; Step 2: preparing a second mixed solution, controlling the temperature of the first mixed solution at 60°C to 75°C, adding tall oil and triisopropanolamine to the first mixed solution, adding defoaming components including modified polydimethylsiloxane, polyether-modified silicone and nonylphenol polyoxyethylene ether and deodorizing components including isothiazolinone, triazine compounds, boric acid esters, polycarboxylic acids, heavy alkylbenzene sulfonates and tall oil amide, and then stirring for 20min to 30min to obtain a second mixed solution; Step 3: preparing a composite solution, mixing the first mixed solution and the second mixed solution for 20 minutes, adding an antibacterial agent, an antioxidant, a buffer and a stabilizer, and stirring for a second time for 20 minutes to obtain a composite solution; Step 4: Finished product, add emulsifier, extreme pressure agent and high base synthetic calcium sulfonate to the composite solution, then stir for 20min~30min, and control the temperature at 40℃~50℃, add polyacid triethanolamine ester for the second time, then stir for 20min~30min, control the temperature at 30℃~40℃ for the second time, add water, then stir for 20min~30min, stop heating and stir for 1.5h~2h, filter after cooling to obtain a semi-synthetic cutting fluid.

[0030] The defoaming component includes one or more of modified polydimethylsiloxane, polyether-modified silicone and nonylphenol polyoxyethylene ether.

[0031] The weight ratio of each component of the defoaming ingredient is 2%-8% of the total weight of modified polydimethylsiloxane, 3%-10% of polyether modified silicone and 5%-10% of nonylphenol polyoxyethylene ether.

[0032] The deodorizing ingredient includes one or more of isothiazolinone, triazine compound, boric acid ester, polycarboxylic acid, heavy alkyl benzene sulfonate and tall oil amide.

[0033] The weight ratio of each component of the deodorizing ingredient is 3%-5% of isothiazolinone, 2%-5% of triazine compounds, 2%-3% of boric acid esters, 5%-10% of polycarboxylic acids, 5%-8% of heavy alkylbenzene sulfonates and 3%-5% of tall oil amide based on the total weight.

[0034] Through the above-mentioned proportions, the cutting fluid prepared in Example 2 and the comparative example has the following advantages: modified polydimethylsiloxane helps the cutting fluid to better wet the metal surface and improve the spreading ability of the liquid, thereby improving the processing accuracy and surface finish; polyether-modified silicone can achieve defoaming and foam suppression of the cutting fluid, and can increase the cooling effect of the cutting fluid, reduce the foam generated by the cutting fluid, and improve the use effect of the cutting fluid; isothiazolinone, triazine compounds, boric acid esters, polycarboxylic acids, heavy alkyl benzene sulfonates and tall oil amide enable the cutting fluid to achieve deodorization and reduce environmental pollution.

[0035] Embodiment 3 Please refer to Figure 1 As shown: A semi-synthetic cutting fluid and a preparation method thereof, comprising the following steps: Step 1: Prepare a first mixed liquid, heat the base oil to 75°C~85°C, and then stir for 20min~30min to obtain a first mixed liquid; Step 2: preparing a second mixed solution, controlling the temperature of the first mixed solution at 60° C. to 75° C., adding tall oil and triisopropanolamine to the first mixed solution, and then stirring for 20 min to 30 min to obtain a second mixed solution; Step 3: preparing a composite solution, mixing the first mixed solution and the second mixed solution for 20 minutes, adding an antibacterial agent, an antioxidant, a buffer and a stabilizer, and then adding a preservation material including pure water, deionized water and phenoxyethanol, and stirring for a second time for 20 minutes to obtain a composite solution; Step 4: Finished product, add emulsifier, extreme pressure agent and high base synthetic calcium sulfonate to the composite solution, then stir for 20min~30min, and control the temperature at 40℃~50℃, add polyacid triethanolamine ester for the second time, then stir for 20min~30min, control the temperature at 30℃~40℃ for the second time, add water, then stir for 20min~30min, stop heating and stir for 1.5h~2h, filter after cooling to obtain a semi-synthetic cutting fluid.

[0036] The antibacterial agent in step 3 is selected from at least one of triazines, isothiazolinones, morpholines or iodopropynyl butylcarbamate; The antioxidant is selected from at least one of triethanolamine, isopropanolamine or diglycolamine; The buffer is selected from at least one of sodium carbonate, sodium bicarbonate, acetic acid, citric acid or ammonia water.

[0037] The quality-preserving materials include pure water, deionized water and phenoxyethanol. The temperature in step three is controlled at 70° C. to 75° C., and the cooling time in step four is 0.3 h to 1 h.

[0038] Through the above-mentioned ratio, the cutting fluid prepared in Example 3 and the comparative example has the following advantages: it can delay the deterioration of the cutting fluid, and phenoxyethanol can ensure the uniformity of the cutting fluid, can quickly take away the heat generated by friction, help maintain the temperature stability of the tool and the workpiece, avoid the loss of precision caused by overheating, and increase the practicality of the cutting fluid.

[0039] The test results of anti-corrosion performance, defoaming rate and shelf life are shown in Table 1 below: Table 1: Tests on anti-corrosion performance, defoaming rate and shelf life:

[0040] It can be seen from the test results in the above table that the semi-synthetic cutting fluid prepared in Example 1 can effectively reduce the friction between the tool and the workpiece, reduce wear, and make the cutting fluid more evenly distributed on the processing surface, thereby optimizing the cooling and cleaning process, so that while ensuring lubrication, it can achieve efficient corrosion protection for mechanical equipment; the semi-synthetic cutting fluid prepared in Example 2 can achieve defoaming and foam suppression of the cutting fluid, increase the cooling effect of the cutting fluid, reduce the foam generated by the cutting fluid, and improve the use effect of the cutting fluid. At the same time, heavy alkyl benzene sulfonate and tall oil amide also make the cutting fluid achieve better deodorization and deodorization effects; the semi-synthetic cutting fluid prepared in Example 3 is compared with the comparative example, phenoxyethanol, phenoxyethanol can prolong the shelf life of the cutting fluid, and can delay the deterioration of the cutting fluid. Therefore, the semi-synthetic cutting fluid prepared in the present invention is worthy of market promotion.

[0041] The present invention provides a semi-synthetic cutting fluid and a preparation method thereof. During operation, the method first heats the base oil to 75°C to 85°C, adds the corrosion-resistant material and the lubricant to the base oil under stirring, and then stirs for 20min to 30min to obtain a first mixed liquid. The foam-free aluminum corrosion inhibitor DX521 and the high molecular synthetic fat make the cutting fluid have low surface tension and high heat resistance, can effectively penetrate the foam film and destroy the foam structure, and the high molecular synthetic fat includes rapeseed oil, which has excellent biodegradability and low toxicity, and provides good environmental protection characteristics and lubricity for the cutting fluid. Nitrite effectively prevents the oxidation reaction of the metal, and triethanolamine has good Physical adsorption and lubricity can effectively reduce the friction between the tool and the workpiece, reduce wear, and make the cutting fluid more evenly distributed on the processing surface, thereby optimizing the cooling and cleaning process, so that while ensuring lubrication, it can achieve efficient corrosion protection for mechanical equipment and reduce corrosion of mechanical equipment; the temperature of the first mixed liquid is controlled at 60℃~75℃, tall oil and triisopropanolamine are added to the first mixed liquid, and defoaming components and deodorizing components are added, and then stirred for 20min~30min to obtain the second mixed liquid. The modified polydimethylsiloxane helps the cutting fluid to better wet the metal surface and improve the spreading ability of the liquid, thereby improving the processing accuracy and surface finish. degree, polyether modified silicone can achieve defoaming and defoaming of cutting fluid, increase the cooling effect of cutting fluid, reduce the foam generated by cutting fluid, and improve the use effect of cutting fluid, isothiazolinone, triazine compounds, boric acid esters, polycarboxylic acids, heavy alkyl benzene sulfonates and tall oil amide, so that the cutting fluid can be deodorized and deodorized, and environmental pollution can be reduced; the first mixed liquid and the second mixed liquid are mixed and stirred for 20 minutes, and antibacterial agents, antioxidants, buffers and stabilizers are added, and then the quality preservation materials are added, and stirred for a second time for 20 minutes to obtain a composite solution, the quality preservation materials include phenoxyethanol, phenoxyethanol can prolong the shelf life of the cutting fluid, and can delay the deterioration of the cutting fluid, and Phenoxyethanol can ensure the uniformity of the cutting fluid, can quickly take away the heat generated by friction, help maintain the temperature stability of the tool and the workpiece, avoid the loss of precision caused by overheating, and increase the practicality of the cutting fluid; add emulsifiers, extreme pressure agents and high-base synthetic calcium sulfonate to the composite solution, then stir for 20min~30min, and control the temperature at 40℃~50℃, add polyacid triethanolamine ester for the second time, and then stir for 20min~30min, control the temperature at 30℃~40℃ for the second time, add water, and then stir for 20min~30min, stop heating and stir for 1.5h~2h, filter after cooling to obtain a semi-synthetic cutting fluid.

[0042] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A semi-synthetic cutting fluid, characterized in that: The preparation method of the semi-synthetic cutting fluid comprises the following steps: Step 1: preparing a first mixed liquid, heating the base oil to 75°C to 85°C, adding the corrosion-resistant material and the lubricant to the base oil under stirring, and then stirring for 20min to 30min to obtain the first mixed liquid; Step 2: preparing a second mixed solution, controlling the temperature of the first mixed solution at 60° C. to 75° C., adding tall oil and triisopropanolamine to the first mixed solution, and adding a defoaming component and a deodorizing component, and then stirring for 20 min to 30 min to obtain a second mixed solution; Step 3: preparing a composite solution, mixing the first mixed solution and the second mixed solution for 20 minutes, adding an antimicrobial agent, an antioxidant, a buffer and a stabilizer, and then adding a shelf-life material, stirring for a second time for 20 minutes to obtain a composite solution; Step 4: Finished product, add emulsifier, extreme pressure agent and high base synthetic calcium sulfonate to the composite solution, then stir for 20min~30min, and control the temperature at 40℃~50℃, add polyacid triethanolamine ester for the second time, then stir for 20min~30min, control the temperature at 30℃~40℃ for the second time, add water, then stir for 20min~30min, stop heating and stir for 1.5h~2h, filter after cooling to obtain a semi-synthetic cutting fluid.

2. The method according to claim 1, characterized in that: The corrosion-resistant material in step 1 includes bubbling-free aluminum corrosion inhibitor DX521, nitrite, triethanolamine and polymer synthetic fat. The weight ratio of each component of the corrosion-resistant material is 1%-5% of the bubbling-free aluminum corrosion inhibitor DX521 and 5%-10% of the polymer synthetic fat based on the total weight.

3. The method according to claim 2, characterized in that The high molecular weight synthetic fat includes rapeseed oil, and the weight ratio of the rapeseed oil is 1%-5% of the total weight.

4. The method according to claim 1, characterized in that: The lubricant comprises one or more combinations of erucamide, graphite, molybdenum disulfide, fatty alcohol polyoxyethylene ether and nitrite; The weight ratio of each component of the lubricant is 2%-8% of erucamide, 2%-5% of graphite, 2%-15% of molybdenum disulfide, 5%-10% of fatty alcohol polyoxyethylene ether and 3%-7% of nitrite based on the total weight.

5. The method according to claim 1, characterized in that The defoaming component includes one or more of modified polydimethylsiloxane, polyether-modified silicone and nonylphenol polyoxyethylene ether.

6. The method according to claim 5, characterized in that The weight ratio of each component of the defoaming component is 2%-8% of the total weight of modified polydimethylsiloxane, 3%-10% of polyether modified silicone and 5%-10% of nonylphenol polyoxyethylene ether.

7. The method according to claim 1, characterized in that The deodorizing component comprises one or more of isothiazolinone, triazine compound, boric acid ester, polycarboxylic acid, heavy alkyl benzene sulfonate and tall oil amide.

8. The method according to claim 7, characterized in that The weight ratio of each component of the deodorizing ingredient is 3%-5% of isothiazolinone, 2%-5% of triazine compounds, 2%-3% of boric acid esters, 5%-10% of polycarboxylic acids, 5%-8% of heavy alkylbenzene sulfonates and 3%-5% of tall oil amide based on the total weight.

9. The method according to claim 1, characterized in that: The antibacterial agent in step 3 is selected from at least one of triazines, isothiazolinones, morpholines or iodopropynyl butylcarbamate; The antioxidant is selected from at least one of triethanolamine, isopropanolamine or diglycolamine; The buffer is selected from at least one of sodium carbonate, sodium bicarbonate, acetic acid, citric acid or ammonia water.

10. The method according to claim 1, characterized in that The quality preservation material includes pure water, deionized water and phenoxyethanol. The temperature in step three is controlled at 70° C. to 75° C., and the cooling time in step four is 0.3 h to 1 h.