Thin film for lubrication as well as preparation method and application of thin film
By coating surface functionalized molybdenum disulfide nanosheets on the DLC film, the problems of poor lubrication effect and insufficient wear resistance of the DLC film in lubricating oil are solved, and higher tribological performance and service life are achieved.
Patent Information
- Application Number
- CN202410986939.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-15
AI Technical Summary
The existing DLC films have poor lubricating effects in lubricating oils and are difficult to form friction chemical reactions with additives, resulting in insufficient wear resistance.
The polyα-olefin oil mixed with diamond film and surface functionalized molybdenum disulfide nanosheets were prepared by ultrasonic dispersion and coating technology, including oleamine, oleic acid, n-octadecyl mercaptan and Molybdenum disulfide nanosheets modified by silane coupling agent enhance the tribological properties of DLC films.
It improves the tribological performance and service life of DLC films, reduces the energy loss of moving parts during friction, enhances the wetting and storage capacity of lubricating oil, and achieves higher wear resistance.
Smart Images

Figure CN118956474A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of lubrication, and in particular to a film for lubrication and a preparation method and application thereof. Background Art
[0002] With the rapid development of science and technology and modern industry, the service environment of mechanical equipment is becoming increasingly complex and demanding. A single lubrication technology may not be able to meet the lubrication requirements of specific working conditions. In recent years, solid-liquid composite lubrication systems have attracted much attention. They are a lubrication method that organically combines solid lubricants and liquid lubricants. This lubrication method can give full play to the high load-bearing capacity of solid lubricants and the excellent lubrication properties of liquid lubricants, thereby improving lubrication efficiency and reducing friction and wear.
[0003] Diamond-like carbon (DLC) films have been widely used in the industrial field due to their excellent mechanical properties (hardness and elastic modulus), tribological properties (low friction and low wear) and chemical stability, including magnetic hard disk drives, molds, tools, bearings, aerospace, mechanical face seals, engine parts, gears, biomedicine and micro-electromechanical systems (MEMS), etc. Therefore, DLC films are generally considered to be the strongest competitors among solid lubricating films. The lubrication effect of a single DLC film is disappointing, and in more serious cases, the DLC film may peel off from the substrate surface. In order to further enhance the lubrication effect of DLC films in lubricating oils, additives are often added to the lubricating oils to construct a DLC-based solid-liquid composite lubrication system. The DLC-based solid-liquid composite lubrication system is mainly composed of DLC films, lubricants and additives. As a solid lubricant, DLC films can effectively reduce the wear between friction pairs. Lubricants can provide continuous lubrication for friction pairs to ensure the normal operation of equipment. Additives are selected according to actual needs, such as nanoparticles, graphene, etc., to further improve the performance of the lubrication system. However, it is difficult for DLC films to undergo tribochemical reactions with most additives to form a friction film.
[0004] Therefore, the reasonable selection of additives compatible with the DLC film is the key to achieving synergistic lubrication between the DLC film and the lubricating oil, and ultimately achieving the wear-resistant behavior of the DLC film. Summary of the invention
[0005] The object of the present invention is to provide a film for lubrication and a preparation method and application thereof, so as to improve the problems existing in the prior art.
[0006] In a first aspect, the present invention provides a film for lubrication, comprising a diamond film and a poly-alpha-olefin oil coated on the surface of the diamond-like film, wherein surface-functionalized molybdenum disulfide nanosheets are uniformly dispersed in the poly-alpha-olefin oil; wherein the surface-functionalized molybdenum disulfide nanosheets include oleylamine surface-functionalized molybdenum disulfide nanosheets, oleic acid surface-functionalized molybdenum disulfide nanosheets, n-octadecyl mercaptan surface-functionalized molybdenum disulfide nanosheets and silane coupling agent surface-functionalized molybdenum disulfide nanosheets.
[0007] In a second aspect, the present invention provides a method for preparing a film for lubrication, which is used to prepare the above-mentioned film, comprising: preparing a diamond film on a steel surface; preparing surface-functionalized molybdenum disulfide nanosheets; uniformly dispersing the surface-functionalized molybdenum disulfide nanosheets in poly-α-olefin oil; uniformly coating the poly-α-olefin oil added with surface-functionalized molybdenum disulfide nanosheets on the surface of the diamond film to obtain a film for lubrication; wherein the preparation of the surface-functionalized molybdenum disulfide nanosheets comprises: preparing oleylamine surface-functionalized molybdenum disulfide nanosheets, preparing oleic acid surface-functionalized molybdenum disulfide nanosheets, preparing n-octadecyl mercaptan surface-functionalized molybdenum disulfide nanosheets, and preparing silane coupling agent surface-functionalized molybdenum disulfide nanosheets.
[0008] More preferably, the diamond film includes an undoped diamond-like film, a tungsten-doped diamond-like film, a titanium-doped diamond-like film or a silicon-doped diamond-like film; poly-α-olefin oil mixed with molybdenum disulfide nanosheets with different surface functionalizations is combined with different diamond films, wherein poly-α-olefin oil mixed with molybdenum disulfide nanosheets with oleylamine surface functionalizations is combined with titanium-doped diamond-like film, poly-α-olefin oil mixed with molybdenum disulfide nanosheets with oleic acid surface functionalizations is combined with an undoped diamond-like film, poly-α-olefin oil mixed with molybdenum disulfide nanosheets with n-octadecyl mercaptan surface functionalizations is combined with tungsten-doped diamond-like film, and poly-α-olefin oil mixed with molybdenum disulfide nanosheets with silane coupling agent surface functionalizations is combined with silicon-doped diamond-like film.
[0009] More preferably, the mass concentration of the surface functionalized molybdenum disulfide nanosheets in the poly-α-olefin oil is 0.5%-4%.
[0010] More preferably, oleylamine surface functionalized molybdenum disulfide nanosheets are prepared, specifically comprising: weighing 0.618-3.09 parts by mass of ammonium molybdate tetrahydrate and 1.14-5.7 parts by mass of thiourea, and adding them into a beaker containing 7-50 parts by mass of oleylamine and 7-50 parts by mass of octadecene mixture; secondly, ultrasonically dispersing it for 20-30 minutes and then continuing to stir at room temperature for 20-30 minutes to mix the reaction solution evenly; then, transferring the above reaction solution to a stainless steel autoclave lined with polytetrafluoroethylene and keeping it at 200°C for 18-20 hours; after naturally cooling to room temperature, filtering, washing and drying to obtain oleylamine-modified MoS2.
[0011] More preferably, oleic acid surface functionalized molybdenum disulfide nanosheets are prepared, specifically comprising: weighing 0.618-3.09 parts by mass of ammonium molybdate tetrahydrate, 1.14-5.7 parts by mass of thiourea and 0.2-1 parts by mass of hydroxylamine hydrochloride, and adding them to a beaker containing 10-50 parts by mass of oleic acid and 20-100 parts by mass of a mixture of water; secondly, ultrasonically dispersing it for 20-30 minutes and then continuing to stir at room temperature for 20-30 minutes to mix the reaction solution evenly; then, transferring the above reaction solution to a stainless steel autoclave lined with polytetrafluoroethylene and keeping it at 200°C for 18-20 hours; after naturally cooling to room temperature, filtering, washing and drying to obtain oleic acid-modified MoS2.
[0012] More preferably, before preparing the n-octadecyl mercaptan surface functionalized molybdenum disulfide nanosheets and the silane coupling agent surface functionalized molybdenum disulfide nanosheets, a solvothermal method is used to prepare unmodified MoS2, specifically comprising: weighing 0.618-3.09 parts by mass of ammonium molybdate tetrahydrate and 1.14-5.7 parts by mass of thiourea, and adding them to a beaker containing 8-50 parts by mass of polyethylene glycol 400 and 8-50 parts by mass of a mixture of deionized water; secondly, ultrasonically dispersing it for 20-30 minutes and then continuing to stir at room temperature for 20-30 minutes to mix the reaction solution evenly; then, transferring the above reaction solution to a stainless steel autoclave lined with polytetrafluoroethylene and keeping it at 200°C for 18-20 hours; after naturally cooling to room temperature, filtering, washing, and drying to obtain unmodified MoS2.
[0013] More preferably, n-octadecyl mercaptan surface functionalized molybdenum disulfide nanosheets are prepared, specifically comprising: ultrasonically mixing 0.2-1 parts by mass of unmodified MoS2 with 100-500 parts by mass of Tris buffer (10mM, pH=8.5) for 10-30 minutes to uniformly disperse MoS2 in the Tris buffer; then adding 0.3-1.5 parts by mass of n-octadecyl mercaptan, stirring at room temperature for 12-15 hours at a stirring speed of 200-500rpm; filtering, washing, and drying to obtain n-octadecyl mercaptan-modified MoS2.
[0014] More preferably, silane coupling agent surface functionalized molybdenum disulfide nanosheets are prepared, specifically comprising: adding 1-5 parts by mass of unmodified MoS2 to 100-500 parts by mass of anhydrous ethanol, ultrasonically mixing for 30-60 minutes to uniformly disperse the MoS2 in the anhydrous ethanol; then adding 0.5-3 parts by mass of silane coupling agent KH550, stirring at room temperature for 3-6 hours at a stirring speed of 400-600rpm; filtering, washing, and drying to obtain MoS2 modified with silane coupling agent KH550.
[0015] In a third aspect, a film for lubrication is used, wherein the film is prepared by any of the above-mentioned preparation methods, and the film for lubrication is applied to the surfaces of two or more mechanical parts in contact with each other.
[0016] Compared with the prior art, the advantages of the present invention are:
[0017] 1. The surface roughness of the undoped DLC film and the DLC film doped with tungsten, titanium or silicon element prepared by the present invention is nanometer-level, which is conducive to the infiltration and storage of lubricating oil. In addition, the film has high mechanical properties and excellent tribological properties.
[0018] 2. The present invention designs MoS2 nanosheets with different surface functionalizations for DLC films with different doping elements, thereby enhancing the tribological properties of the DLC films.
[0019] 3. The MoS2 nanosheets used in the present invention have excellent tribological properties, which can reduce the energy loss of moving parts during the friction process and increase the service life of moving parts. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is the infrared spectrum of oleic acid modified MoS2 prepared in the present invention.
[0021] Figure 2 This is the infrared spectrum of n-octadecyl mercaptan-modified MoS2 prepared in the present invention.
[0022] Figure 3 This is the infrared spectrum of oleylamine-modified MoS2 prepared in the present invention.
[0023] Figure 4 This is the infrared spectrum of MoS2 modified by the silane coupling agent KH550 prepared in the present invention.
[0024] Figure 5 The friction coefficient and wear rate results of the solid-liquid composite lubrication system constructed by the undoped DLC film prepared by the present invention, the DLC film doped with tungsten, titanium or silicon elements, poly-α-olefin oil and MoS2 nanosheets with different surface functionalizations.
[0025] Figure 6 The friction coefficient and wear rate results of the solid-liquid composite lubrication system constructed by the undoped DLC film prepared by the present invention, the DLC film doped with tungsten, titanium or silicon elements, poly-α-olefin oil and unmodified MoS2 nanosheets.
[0026] Figure 7 A three-dimensional morphology image of the wear scar of a solid-liquid composite lubrication system constructed using the titanium DLC film prepared in the present invention, poly-α-olefin oil, and oleylamine surface functionalized MoS2 nanosheets.
[0027] Figure 8 SEM image of wear scars of a solid-liquid composite lubrication system constructed using the titanium DLC film prepared in the present invention, poly-α-olefin oil, and oleylamine surface functionalized MoS2 nanosheets. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be understood by people with general skills in the field to which the present invention belongs. "Including" and similar words used in this article mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects.
[0029] An embodiment of the present invention provides a film for lubrication, comprising a diamond film and a poly-alpha-olefin oil coated on the surface of the diamond-like film, wherein surface-functionalized molybdenum disulfide nanosheets are uniformly dispersed in the poly-alpha-olefin oil; wherein the surface-functionalized molybdenum disulfide nanosheets include oleylamine surface-functionalized molybdenum disulfide nanosheets, oleic acid surface-functionalized molybdenum disulfide nanosheets, n-octadecyl mercaptan surface-functionalized molybdenum disulfide nanosheets, and silane coupling agent surface-functionalized molybdenum disulfide nanosheets.
[0030] The present invention also provides a method for preparing a lubricating film, which is used to prepare a lubricating film. Figure 1-Figure 8As shown, it includes: using a magnetron sputtering deposition system to prepare a diamond film on the surface of A1SI52100 steel; preparing surface-functionalized molybdenum disulfide nanosheets; uniformly dispersing the surface-functionalized molybdenum disulfide nanosheets in polyalphaolefin oil by ultrasonic dispersion; uniformly coating the polyalphaolefin oil added with surface-functionalized molybdenum disulfide nanosheets on the surface of the diamond film, and ensuring that the polyalphaolefin oil can completely cover the friction surface of the diamond film to obtain a film for lubrication; wherein, preparing the surface-functionalized molybdenum disulfide nanosheets includes: preparing oleylamine surface-functionalized molybdenum disulfide nanosheets, preparing oleic acid surface-functionalized molybdenum disulfide nanosheets, preparing n-octadecyl mercaptan surface-functionalized molybdenum disulfide nanosheets, and preparing silane coupling agent surface-functionalized molybdenum disulfide nanosheets.
[0031] In some embodiments, the diamond film includes an undoped diamond-like film, a tungsten-doped diamond-like film, a titanium-doped diamond-like film or a silicon-doped diamond-like film; poly-α-olefin oil mixed with molybdenum disulfide nanosheets with different surface functionalizations is combined with different diamond films, wherein poly-α-olefin oil mixed with molybdenum disulfide nanosheets with oleylamine surface functionalizations is combined with titanium-doped diamond-like film, poly-α-olefin oil mixed with molybdenum disulfide nanosheets with oleic acid surface functionalizations is combined with an undoped diamond-like film, poly-α-olefin oil mixed with molybdenum disulfide nanosheets with n-octadecyl mercaptan surface functionalizations is combined with tungsten-doped diamond-like film, and poly-α-olefin oil mixed with molybdenum disulfide nanosheets with silane coupling agent surface functionalizations is combined with silicon-doped diamond-like film.
[0032] In some embodiments, the mass concentration of the surface functionalized molybdenum disulfide nanosheets in the poly-alpha-olefin oil is 0.5%-4%.
[0033] An embodiment of the present invention further provides an application of a thin film for lubrication, wherein the thin film for lubrication is applied to the surfaces of two or more mechanical parts in contact with each other.
[0034] Specifically, the lubricating film prepared by the poly-α-olefin oil mixed with the different diamond films and the different surface functionalized molybdenum disulfide nanosheets in the above embodiment was tested, and the friction test was carried out using a UMT-5 reciprocating friction and wear testing machine. The experimental load was 20N, the sliding frequency was 4Hz, the stroke was 5mm, and the test time was 30min. The specific experimental method and experimental results are as follows.
[0035] Embodiment 1:
[0036] (1) Using a magnetron sputtering deposition system, an undoped DLC film was prepared on the surface of AISI52100 steel. The surface roughness of the undoped DLC film was measured by atomic force microscopy to be 5.21 nm, the thickness was measured by scanning electron microscopy to be 2.1 μm, and the hardness and elastic modulus were measured by nanoindentation to be 14.29 GPa and 160.77 GPa, respectively.
[0037] (2) Preparation of MoS2 with surface modified with oleic acid, the specific steps are as follows: weigh 1.236g of ammonium molybdate tetrahydrate, 2.28g of thiourea and 0.5g of hydroxylamine hydrochloride, add them to a beaker containing a mixture of 20mL of oleic acid and 30mL of deionized water; secondly, ultrasonically disperse it for 20min and continue stirring at room temperature for 20min to mix the reaction solution evenly; then, transfer the above reaction solution to a 100mL polytetrafluoroethylene-lined stainless steel autoclave and keep it at 200℃ for 18h; after cooling naturally to room temperature, filter, wash and dry to obtain oleic acid-modified MoS2. Its infrared spectrum is shown in the figure below: Figure 1 As shown. At 3433, 2914, 2846, 1626, 1412, 1093 and 934cm -1 The peak that appears nearby is the infrared characteristic peak of oleic acid, indicating that the MoS2 surface is modified with oleic acid molecules.
[0038] (3) A ball and a disk coated with an undoped DLC film were selected as the upper and lower friction pairs of the friction experiment. The friction experiment was carried out using a UMT-5 reciprocating friction and wear tester. Polyalphaolefin oil with 3% MoS2 nanosheets added was dropped on the surface of the undoped DLC film by manual coating, so that the lubricating oil could completely cover the friction surface. The experimental load was 20N, the sliding frequency was 4Hz, the stroke was 5mm, and the test time was 30min. Figure 5 It can be seen that the friction coefficient is 0.084 and the wear rate is 9.1×10 - 9 mm 3 / Nm.
[0039] Embodiment 2:
[0040] (1) Using a magnetron sputtering deposition system, a tungsten-doped DLC film was prepared on the surface of AISI52100 steel. The tungsten-doped DLC film prepared in this example had a surface roughness of 7.26 nm, a thickness of 2.4 μm, and hardness and elastic modulus of 13.14 GPa and 136.58 GPa, respectively. The test method was the same as in Example 1.
[0041] (2) Preparation of MoS2 surface modified with n-octadecyl mercaptan. The specific synthesis steps are as follows: 200 mg MoS2 and 100 mL Tris buffer (10 mM, pH = 8.5) were ultrasonically mixed for 10 min to uniformly disperse MoS2 in the Tris buffer; then 300 mg n-octadecyl mercaptan was added and stirred at room temperature for 12 h at a stirring speed of 200 rpm; filtered, washed, and dried to obtain n-octadecyl mercaptan-modified MoS2. Its infrared spectrum is shown in the figure below. Figure 2 As shown. At 3426, 2920, 2846, 1466, 1018 and 715cm -1 The peak that appears nearby is the infrared characteristic peak of n-octadecyl mercaptan, indicating that the surface of MoS2 is modified with n-octadecyl mercaptan molecules.
[0042] (3) A ball and a disk coated with a tungsten-doped DLC film were selected as the upper and lower friction pairs of the friction experiment. The friction experiment was carried out using a UMT-5 reciprocating friction and wear tester. The poly-α-olefin oil with 0.5% MoS2 nanosheets added was dropped on the surface of the tungsten-doped DLC film by manual coating, so that the lubricating oil could completely cover the friction surface. The experimental load was 20N, the sliding frequency was 4Hz, the stroke was 5mm, and the test time was 30min. Figure 5 It can be seen that the friction coefficient is 0.079 and the wear rate is 8.1×10 -9 mm 3 / Nm.
[0043] Embodiment 3:
[0044] (1) A titanium-doped DLC film was prepared on the surface of AISI52100 steel using a magnetron sputtering deposition system. The titanium-doped DLC film prepared in this example had a surface roughness of 7.68 nm, a thickness of 2.6 μm, and hardness and elastic modulus of 9.35 GPa and 95.41 GPa, respectively. The test method was the same as in Example 1.
[0045] (2) Preparation of MoS2 with surface modified with oleylamine. The specific synthesis steps are as follows: weigh 1.236g of ammonium molybdate tetrahydrate and 2.28g of thiourea, add them into a beaker containing 15mL of oleylamine and 15mL of octadecene mixture; secondly, ultrasonically disperse it for 20min and continue stirring at room temperature for 20min to mix the reaction solution evenly; then, transfer the reaction solution to a 100mL polytetrafluoroethylene-lined stainless steel autoclave and keep it at 200℃ for 18h; after cooling naturally to room temperature, filter, wash and dry to obtain oleylamine-modified MoS2. Its infrared spectrum is shown in the figure below. Figure 3 As shown, at 2917, 2847, 1648, 1621, 1403 and 720 cm -1The peak that appears nearby is the infrared characteristic peak of oleylamine, indicating that the MoS2 surface is modified with oleylamine molecules.
[0046] (3) A ball and a disk coated with a titanium-doped DLC film were selected as the upper and lower friction pairs of the friction experiment. The friction experiment was carried out using a UMT-5 reciprocating friction and wear tester. The poly-α-olefin oil with 4% MoS2 nanosheets added was dropped on the surface of the titanium-doped DLC film by manual coating, so that the lubricating oil could completely cover the friction surface. The experimental load was 20N, the sliding frequency was 4Hz, the stroke was 5mm, and the test time was 30min. Figure 5 It can be seen that the friction coefficient is 0.073 and the wear rate is 9.8×10 -9 mm 3 / Nm.
[0047] Through white light interferometry ( Figure 6 ) and SEM ( Figure 7 ) The wear mark analysis shows that the worn surface is relatively smooth and no obvious scratches are found. It can be seen that the present invention provides a wear-resistant solid-liquid composite lubrication system.
[0048] Embodiment 4:
[0049] (1) A silicon-doped DLC film was prepared on the surface of AISI52100 steel using a magnetron sputtering deposition system. The silicon-doped DLC film prepared in this example had a surface roughness of 4.62 nm, a thickness of 2.8 μm, and hardness and elastic modulus of 8.51 GPa and 83.59 GPa, respectively. The test method was the same as in Example 1.
[0050] (2) Preparation of MoS2 surface modified with silane coupling agent KH550. The specific synthesis steps are as follows: add 1g MoS2 to 100g anhydrous ethanol, and mix by ultrasonic for 30min to make MoS2 evenly dispersed in anhydrous ethanol; then add 0.5g silane coupling agent KH550, stir at room temperature for 3h, and the stirring speed is 400rpm; filter, wash, and dry to obtain MoS2 modified with silane coupling agent KH550. Its infrared spectrum is shown in the figure below: Figure 4 As shown. At 3384, 3006, 2892, 1604, 1400 and 1107cm -1 The peak that appears nearby is the infrared characteristic peak of silane coupling agent KH550, indicating that the MoS2 surface is modified with silane coupling agent KH550 molecules.
[0051] (3) A ball and a disk coated with a silicon-doped DLC film were selected as the upper and lower friction pairs of the friction experiment. The friction experiment was carried out using a UMT-5 reciprocating friction and wear tester. The poly-α-olefin oil with 2% MoS2 nanosheets added was dropped on the surface of the silicon-doped DLC film by manual coating, so that the lubricating oil could completely cover the friction surface. The experimental load was 20N, the sliding frequency was 4Hz, the stroke was 5mm, and the test time was 30min. Figure 5 It can be seen that the friction coefficient is 0.071 and the wear rate is 1.62×10 -8 mm 3 / Nm.
[0052] Comparative Example 1:
[0053] (1) Using a magnetron sputtering deposition system, an undoped DLC film was prepared on the surface of AISI52100 steel. The surface roughness of the undoped DLC film prepared in this comparative example was 5.34 nm, the thickness of the film was 2.06 μm, and the hardness and elastic modulus were 13.79 GPa and 156.21 GPa, respectively. The test method was the same as in Example 1.
[0054] (2) A ball and a disk coated with an undoped DLC film were selected as the upper and lower friction pairs of the friction experiment. The friction experiment was carried out using a UMT-5 reciprocating friction and wear tester. The poly-α-olefin oil with 3% unmodified MoS2 nanosheets was dropped on the surface of the undoped DLC film by manual coating, so that the lubricating oil could completely cover the friction surface. The experimental load was 20N, the sliding frequency was 4Hz, the stroke was 5mm, and the test time was 30min. Figure 6 It can be seen that the friction coefficient is 0.091 and the wear rate is 1.03×10 -8 mm 3 / Nm.
[0055] Comparative Example 2:
[0056] (1) A tungsten-doped DLC film was prepared on the surface of AISI52100 steel using a magnetron sputtering deposition system. The tungsten-doped DLC film prepared in this comparative example had a surface roughness of 7.88 nm, a thickness of 2.33 μm, and hardness and elastic modulus of 12.83 GPa and 130.77 GPa, respectively. The test method was the same as in Example 1.
[0057] (2) A ball and a disk coated with a tungsten-doped DLC film on the surface were selected as the upper and lower friction pairs of the friction experiment. The friction experiment was carried out using a UMT-5 reciprocating friction and wear tester. The poly-α-olefin oil with 0.5% unmodified MoS2 nanosheets was dropped on the surface of the tungsten-doped DLC film by manual coating, so that the lubricating oil could completely cover the friction surface. The experimental load was 20N, the sliding frequency was 4Hz, the stroke was 5mm, and the test time was 30min. Figure 6 It can be seen that the friction coefficient is 0.087 and the wear rate is 9.5×10 -9 mm 3 / Nm.
[0058] Comparative Example 3:
[0059] (1) A titanium-doped DLC film was prepared on the surface of AISI52100 steel using a magnetron sputtering deposition system. The titanium-doped DLC film prepared in this comparative example had a surface roughness of 8.34 nm, a thickness of 2.49 μm, and hardness and elastic modulus of 8.35 GPa and 92.57 GPa, respectively. The test method was the same as in Example 1.
[0060] (2) A ball and a disk coated with a titanium-doped DLC film were selected as the upper and lower friction pairs of the friction experiment. The friction experiment was carried out using a UMT-5 reciprocating friction and wear tester. The poly-α-olefin oil with 4% unmodified MoS2 nanosheets was dropped on the surface of the titanium-doped DLC film by manual coating, so that the lubricating oil could completely cover the friction surface. The experimental load was 20N, the sliding frequency was 4Hz, the stroke was 5mm, and the test time was 30min. Figure 6 It can be seen that the friction coefficient is 0.084 and the wear rate is 1.26×10 -8 mm 3 / Nm.
[0061] Comparative Example 4:
[0062] (1) A silicon-doped DLC film was prepared on the surface of AISI52100 steel using a magnetron sputtering deposition system. The silicon-doped DLC film prepared in this comparative example had a surface roughness of 4.73 nm, a thickness of 2.71 μm, and hardness and elastic modulus of 8.11 GPa and 80.27 GPa, respectively. The test method was the same as in Example 1.
[0063] (2) A ball and a disk coated with a silicon-doped DLC film were selected as the upper and lower friction pairs of the friction experiment. The friction experiment was carried out using a UMT-5 reciprocating friction and wear tester. The poly-α-olefin oil with 2% unmodified MoS2 nanosheets was dropped on the surface of the silicon-doped DLC film by manual coating, so that the lubricating oil could completely cover the friction surface. The experimental load was 20N, the sliding frequency was 4Hz, the stroke was 5mm, and the test time was 30min. Figure 6 It can be seen that the friction coefficient is 0.077 and the wear rate is 3.14×10 -8 mm 3 / Nm.
[0064] Table 1 Performance test results of the film
[0065]
[0066] As can be seen from Table 1 above, the surface roughness, film thickness, hardness and elastic modulus of the films in Examples 1-4 are better than those in Comparative Examples 1-4, and are applicable in the industrial field.
[0067] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.
Claims
1. A film for lubrication, characterized in that: The invention comprises a diamond film and a poly-alpha-olefin oil coated on the surface of the diamond-like film, wherein surface-functionalized molybdenum disulfide nanosheets are uniformly dispersed in the poly-alpha-olefin oil; wherein the surface-functionalized molybdenum disulfide nanosheets comprise oleylamine surface-functionalized molybdenum disulfide nanosheets, oleic acid surface-functionalized molybdenum disulfide nanosheets, n-octadecyl mercaptan surface-functionalized molybdenum disulfide nanosheets and silane coupling agent surface-functionalized molybdenum disulfide nanosheets.
2. A method for preparing a film for lubrication, for preparing the film as claimed in claim 1, characterized in that: include: A diamond film was prepared on the steel surface; Surface functionalized MoS2 nanosheets were prepared; The surface-functionalized MoS2 nanosheets were uniformly dispersed in poly-α-olefin oil; The poly-alpha-olefin oil added with surface functionalized molybdenum disulfide nanosheets is uniformly coated on the surface of the diamond film to obtain a film for lubrication; Among them, the preparation of surface functionalized molybdenum disulfide nanosheets includes: preparing oleylamine surface functionalized molybdenum disulfide nanosheets, preparing oleic acid surface functionalized molybdenum disulfide nanosheets, preparing n-octadecyl mercaptan surface functionalized molybdenum disulfide nanosheets, and preparing silane coupling agent surface functionalized molybdenum disulfide nanosheets.
3. A method for preparing a lubricating film according to claim 2, characterized in that: The diamond film includes an undoped diamond-like film, a tungsten-doped diamond-like film, a titanium-doped diamond-like film or a silicon-doped diamond-like film; poly-α-olefin oil mixed with molybdenum disulfide nanosheets with different surface functionalizations is combined with different diamond films, wherein poly-α-olefin oil mixed with molybdenum disulfide nanosheets with oleylamine surface functionalizations is combined with a titanium-doped diamond-like film, poly-α-olefin oil mixed with molybdenum disulfide nanosheets with oleic acid surface functionalizations is combined with an undoped diamond-like film, poly-α-olefin oil mixed with molybdenum disulfide nanosheets with n-octadecyl mercaptan surface functionalizations is combined with a tungsten-doped diamond-like film, and poly-α-olefin oil mixed with molybdenum disulfide nanosheets with silane coupling agent surface functionalizations is combined with a silicon-doped diamond-like film.
4. A method for preparing a lubricating film according to claim 2, characterized in that: The mass concentration of the surface functionalized molybdenum disulfide nanosheets in the poly-alpha-olefin oil is 0.5%-4%.
5. A method for preparing a lubricating film according to claim 2, characterized in that: The method comprises the following steps: weighing 0.618-3.09 parts by weight of ammonium molybdate tetrahydrate and 1.14-5.7 parts by weight of thiourea, and adding the mixture into a beaker containing 7-50 parts by weight of a mixture of oleylamine and 7-50 parts by weight of octadecene; secondly, ultrasonically dispersing the mixture for 20-30 minutes and then stirring the mixture at room temperature for 20-30 minutes to mix the reaction mixture evenly; then, transferring the reaction mixture into a stainless steel autoclave lined with polytetrafluoroethylene and maintaining the mixture at 200°C for 18-20 hours; and naturally cooling the mixture to room temperature, filtering, washing and drying the mixture to obtain oleylamine-modified MoS2.
6. A method for preparing a lubricating film according to claim 2, characterized in that: The method comprises the following steps: weighing 0.618-3.09 parts by weight of ammonium molybdate tetrahydrate, 1.14-5.7 parts by weight of thiourea and 0.2-1 parts by weight of hydroxylamine hydrochloride, and adding the mixture into a beaker containing 10-50 parts by weight of oleic acid and 20-100 parts by weight of a water mixture; secondly, ultrasonically dispersing the mixture for 20-30 minutes, and then stirring the mixture at room temperature for 20-30 minutes to uniformly mix the reaction mixture; then, transferring the reaction mixture into a stainless steel autoclave lined with polytetrafluoroethylene, and maintaining the mixture at 200°C for 18-20 hours; and naturally cooling the mixture to room temperature, filtering, washing and drying the mixture to obtain oleic acid-modified MoS2.
7. A method for preparing a lubricating film according to claim 2, characterized in that: Before preparing the n-octadecyl mercaptan surface functionalized molybdenum disulfide nanosheets and the silane coupling agent surface functionalized molybdenum disulfide nanosheets, a solvothermal method is used to prepare unmodified MoS2, which specifically includes: Weigh 0.618-3.09 parts by mass of ammonium molybdate tetrahydrate and 1.14-5.7 parts by mass of thiourea, and add them into a beaker containing 8-50 parts by mass of polyethylene glycol 400 and 8-50 parts by mass of a mixture of deionized water; secondly, ultrasonically disperse it for 20-30 minutes and continue stirring at room temperature for 20-30 minutes to mix the reaction solution evenly; then, transfer the above reaction solution to a stainless steel autoclave lined with polytetrafluoroethylene and keep it at 200°C for 18-20 hours; after naturally cooling to room temperature, filter, wash and dry to obtain unmodified MoS2.
8. A method for preparing a lubricating film according to claim 7, characterized in that: The method comprises the following steps: ultrasonically mixing 0.2-1 parts by weight of unmodified MoS2 with 100-500 parts by weight of Tris buffer for 10-30 minutes, wherein the concentration of the Tris buffer is 10 mM and the pH value is 8.5, so that the MoS2 is evenly dispersed in the Tris buffer; then, 0.3-1.5 parts by weight of n-octadecyl mercaptan are added, and the mixture is stirred at room temperature for 12-15 hours at a stirring speed of 200-500 rpm; and filtering, washing and drying are performed to obtain n-octadecyl mercaptan-modified MoS2.
9. A method for preparing a lubricating film according to claim 7, characterized in that: The method comprises the following steps: adding 1-5 parts by weight of unmodified MoS2 to 100-500 parts by weight of anhydrous ethanol, and ultrasonically mixing the unmodified MoS2 for 30-60 minutes to uniformly disperse the MoS2 in the anhydrous ethanol; then adding 0.5-3 parts by weight of a silane coupling agent, and stirring the unmodified MoS2 at room temperature for 3-6 hours at a stirring speed of 400-600 rpm; and filtering, washing, and drying the unmodified MoS2.
10. An application of a film for lubrication, wherein the film is prepared by the method according to any one of claims 2 to 9, characterized in that: Applying a thin film for lubrication to the surfaces of two or more mechanical parts in contact with each other.
Citation Information
Cited By
Friction matching pair system, preparation method and method for realizing ultra-low friction of ultra-hard carbon film
CN121592989A