Novel 18Ni300 martensite heat treatment process

By combining solid solution treatment and aging treatment, multiple temperature and time parameters are set, the heat treatment process of 18Ni300 martensite is optimized, which solves the problem that temperature and time are difficult to discuss separately during the aging process, and improves the hardness and forming quality of the material .

CN118957220APending Publication Date: 2024-11-15SUZHOU RONGZHI 3D TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411178609.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

During the aging process of the existing 18Ni300 martensite mold steel, the aging temperature and aging time are difficult to discuss separately, which affects the forming quality and mechanical properties, and there are problems with phase change processing.

Method used

Using the new 18Ni300 martensite heat treatment process, combining solid solution treatment and aging treatment, multiple temperature gears and insulation time are set, and the hardness is detected through furnace cooling and air cooling to obtain the best treatment parameters, including solid Temperature and time settings for dissolution and aging treatment.

Benefits of technology

The hardness of the 18Ni300 composite material is effectively improved, the internal mass and mechanical properties of the formed parts are optimized, the problem of separate discussion of aging temperature and time is solved, and the hardness is maximized.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957220A_ABST
    Figure CN118957220A_ABST
Patent Text Reader

Abstract

The invention discloses a heat treatment process of novel 18Ni300 martensite. Comprising the following steps: S1, setting a heat treatment mode of the 18Ni300 composite material; s2, setting a heat treatment item; s3, setting the temperature of heat treatment; s4, setting the duration of heat treatment; s5, setting a cooling mode of heat treatment; s6, the hardness of the 18Ni300 composite material is detected; according to the method, single-factor tests are set for solid solution treatment and aging treatment respectively, it is found that in solid solution treatment and aging treatment, the hardness is firstly increased and then reduced along with increasing of temperature and time, and the hardness peak value serves as a better parameter of solid solution treatment and aging treatment; the maximum hardness reaches 380.23 HV at the temperature of 800 DEG C through solution treatment, and when the time-effect temperature is 440 DEG C, the hardness peak value is 536.5 HV; solution treatment 800 DEG C / 1 h and aging treatment 440 DEG C / 3 h are adopted as better heat treatment parameters of solution treatment and aging treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal additive manufacturing, and specifically relates to a novel heat treatment process for 18Ni300 martensite. Background Art

[0002] Since entering the era of Industry 4.0, additive manufacturing technology has ushered in rapid development as a high-end digital and automated manufacturing technology. Compared with the traditional material processing method - cutting processing, additive manufacturing is a technical method to manufacture high-end precision parts by adding materials layer by layer from "bottom to top" (that is, adding materials to parts from points to surfaces and then to layers through slicing programs in three-dimensional space). Additive manufacturing technology adopts the "discrete-superposition" principle, takes the CAD / CAM digital model as the basic file, and uses the "model layering, layer by layer addition" operation method to form three-dimensional parts from powdered metal raw materials, ceramics and polymer materials in a molten sintering state. Additive manufacturing technology combines material preparation with component manufacturing to eliminate subsequent tedious and complex machining steps. In terms of optimizing SLM technology, in addition to optimizing laser process parameters, some experts and scholars have optimized the heat treatment process during SLM post-processing. The heat treatment mechanism of 18Ni300 martensitic die steel is generally divided into three types: solid solution treatment, solid solution plus aging treatment, and direct aging treatment. However, the heat treatment of materials obtained by different preparation methods also has different differences. It can be seen that the heat treatment results of 18Ni300 martensitic die steel need to be compared, and then a targeted heat treatment plan for SLM formed parts should be further formulated. Therefore, it is of certain theoretical significance and application value to carry out theoretical and experimental research on the influence of heat treatment on forming quality during selective laser melting.

[0003] Heat treatment is a common post-processing method for selective laser melting, which can effectively affect the internal quality, mechanical properties and service safety of the final formed parts. Figure 3 As shown in the figure, before 610℃ and after 740℃, when the temperature increases, the phase transformation of 18Ni300 sample is linear. This is because it is α-Fe at lower temperature and γ-Fe at higher temperature. Austenite reaction occurs at higher temperature, and this phase transformation is not achieved overnight, but the temperature changes every second in the range of 610℃ to 748℃. Therefore, it is judged that the starting temperature of austenite phase transformation of 18Ni300 alloy is 610℃, and the ending temperature of phase transformation is 748℃. However, various phase transformation treatments on the market still have various problems.

[0004] For example, a heat treatment process for C250 maraging steel disclosed in the authorization announcement number CN118207395A realizes that the heat treatment process for C250 maraging steel can achieve grain refinement and homogenization of large-size C250 maraging steel, thereby extending the service life of C250 maraging steel. However, it does not solve the problem that the existing 18Ni300 martensitic phase transformation is significantly affected by the aging temperature and aging time during the aging process. Therefore, when discussing the aging system, the aging temperature and aging time cannot be discussed separately. For this reason, we propose a new heat treatment process for 18Ni300 martensite. Summary of the invention

[0005] The purpose of the present invention is to provide a novel heat treatment process for 18Ni300 martensite to solve the problems raised in the above background technology.

[0006] To achieve the above object, the present invention provides the following technical solution: a novel heat treatment process for 18Ni300 martensite, comprising the following steps: S1. Setting a heat treatment method for the 18Ni300 composite material: performing a solid solution treatment and an aging treatment on the 18Ni300 composite material, and achieving heat treatment on the 18Ni300 composite material by combining the solid solution treatment and the aging treatment; S2. Set heat treatment items: set heating temperature and holding time for solution treatment and aging treatment respectively, and set cooling method, including furnace cooling and air cooling; S3. Setting the temperature of heat treatment: There are four temperature levels for the heating temperature of solution treatment and four temperature levels for the heating temperature of aging treatment; S4. Set the duration of heat treatment: the heating duration of solution treatment is set to 1h, and the heating duration of aging treatment includes 1h, 2h, 3h and 4h; S5. Set the cooling method for heat treatment: the cooling method for solution treatment is furnace cooling, and the cooling method for aging treatment is air cooling; S6. Detect the hardness of the 18Ni300 composite material: Detect the hardness of the 18Ni300 composite material through a hardness detection device to obtain the best solution treatment and aging treatment to maximize the hardness of the 18Ni300 composite material.

[0007] Furthermore, the four temperature levels of the solution treatment are set to 750°C, 800°C, 850°C and 900°C, and the corresponding holding times are set to 1h, 1h, 1h and 1h, respectively.

[0008] Further, the four temperature levels of the aging treatment are respectively set to 400° C., 440° C., 480° C. and 520° C., and the four temperature levels of the holding time are respectively set to 1 h, 2 h, 3 h and 4 h; In order to make the temperature and holding time of aging treatment correspond to each other, 8 temperature groups are set, namely 400℃, 440℃, 480℃, 520℃, 440℃, 440℃, 440℃ and 440℃, and the corresponding holding times are 3h, 3h, 3h, 3h, 1h, 2h, 3h and 4h.

[0009] Furthermore, before the heat treatment of the 18Ni300 composite material, the 18Ni300 composite material is preheated, that is, the 18Ni300 composite material is preheated to 600°C at a heating rate of 200-300°C / h, and the 18Ni300 composite material is preheated and kept warm for 10 minutes, and then heated to a treatment temperature of 750°C at a heating rate of 50°C / h, and kept warm for 1 hour, and then subjected to multiple solution treatments, respectively at 750°C, 800°C, 850°C and 900°C.

[0010] Furthermore, the solution treatment is carried out by furnace cooling, wherein high-purity Ar gas is introduced into the furnace, and the Ar pressure is 60-80 MPa; specifically, it is rapidly cooled to room temperature at a cooling rate of 5-10°C / s, and then the hardness of the 18Ni300 composite material is measured.

[0011] Furthermore, the hardness parameters of the 18Ni300 composite material after the solution treatment are as follows: The heating temperature is 750℃, the holding time is 1h, and the furnace cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 375HV. The heating temperature is 800℃, the holding time is 1h, and the furnace cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 380.23HV. The heating temperature is 850℃, the holding time is 1h, and the furnace cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 317.7HV. The heating temperature is 900℃, the holding time is 1h, and the furnace cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 301.57HV. The hardness of the samples of 18Ni300 composite materials showed a trend of first increasing and then decreasing, that is, the 18Ni300 composite material obtained a high-strength and tough lath martensite matrix during the solid solution process, which refined the recrystallized grains produced during the solid solution process, forming a good synergistic effect with the solid solution of metal elements, and reached a maximum hardness of 380.23HV at 800℃. However, judging from the change in hardness before and after the solid solution, the overall hardness of the alloy decreased with increasing temperature.

[0012] Furthermore, after the 18Ni300 composite material is subjected to solution treatment, the 18Ni300 composite material is subjected to aging treatment again; The 18Ni300 composite material is firstly preheated, that is, the 18Ni300 composite material is preheated to 300°C at a heating rate of 50-100°C / h, and the 18Ni300 composite material is preheated and kept warm for 10 minutes, and then heated to a treatment temperature of 400°C at a heating rate of 40°C / h, and kept warm for 3 hours, and then subjected to multiple aging treatments, aging treatments are carried out at 440°C, 480°C and 520°C respectively, and at a temperature of 440°C, the holding time is 1h, 2h, 3h and 4h respectively, and at temperatures of 480°C and 520°C, the holding time is 3h.

[0013] Furthermore, the aging treatment is performed by air cooling, and the air cooling is to place the 18Ni300 composite material at room temperature for slow cooling; and a fan is used to blow air on the 18Ni300 composite material so that the 18Ni300 composite material is cooled to room temperature at a cooling rate of 1-3°C / s, and then the hardness of the 18Ni300 composite material is measured.

[0014] Furthermore, the hardness parameters of the 18Ni300 composite material after aging treatment are as follows: The heating temperature is 400℃, the holding time is 3h, and the air cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 529.27HV. The heating temperature is 440℃, the holding time is 1h, and the air cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 536.17HV. The heating temperature is 440℃, the holding time is 2h, and the air cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 532.07HV. The heating temperature is 440℃, the holding time is 3h, and the air cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 536.5HV. The heating temperature is 440℃, the holding time is 4h, and the air cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 509.63HV. The heating temperature is 480℃, the holding time is 3h, and the air cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 511HV. The heating temperature is 520°C, the holding time is 3h, and air cooling is adopted. The hardness of the treated 18Ni300 composite material is 516.4HV.

[0015] Furthermore, the hardness of the 18Ni300 composite material under different aging temperatures first increases and then decreases. When the aging temperature is 440°C, the hardness of the 18Ni300 composite material reaches a peak value of 536.5HV; that is, increasing the temperature can accelerate the aging precipitation process, and can accelerate the enrichment of the metal, accelerate the nucleation and growth of the metal, and improve the hardness of the 18Ni300 composite material; When the holding time gradually increases, the hardness remains basically unchanged before the aging peak appears, but it is greatly improved compared with the hardness of solution treatment. The amplitude modulation decomposition and precipitation of the aging phase occurs in a very short time, and the lattice distortion increases after precipitation; the hardness basically does not change between 1-2 hours at the beginning of aging, but the hardness changes between 2-3 hours, that is, the hardness increases during this time; however, after 2-3 hours, the hardness begins to gradually decrease in the later stage of aging; that is, when the temperature is maintained at a certain temperature, the accumulated heat will produce reversed austenite; after aging treatment at 440℃ / 3h, the hardness of 18Ni300 composite material is the highest, 440℃ is selected as the aging temperature, and 3 hours is the optimal aging time; solution treatment at 800℃ / 1h and aging treatment at 440℃ / 3h are adopted as the optimal heat treatment parameters for solution treatment and aging treatment.

[0016] Compared with the prior art, the present invention has the following beneficial effects: The heat treatment of the present invention is a commonly used post-treatment method of selective laser melting, which can effectively affect the internal quality, mechanical properties and service safety of the final formed parts. According to the phase change temperature range of the existing 18Ni300 die steel, single factor tests are set for solid solution and aging respectively. It is found that in the solid solution and aging treatment, the hardness first increases and then decreases with the increase of temperature and time, and the hardness peak is used as the optimal parameter of solid solution and aging. During the solution treatment, the hardness of the sample of 18Ni300 composite material showed a trend of first increasing and then decreasing, that is, the 18Ni300 composite material obtained a high-strength and tough lath martensite matrix during the solution process, which made the recrystallized grains produced during the solution process refined, forming a good synergistic effect with the solution of metal elements, and reached a maximum hardness of 380.23HV at 800℃. However, from the change of hardness before and after the solution treatment, the overall hardness of the alloy decreased with the increase of temperature. During aging treatment, the hardness under the aging temperature first increases and then decreases. When the aging temperature is 440℃, the hardness of the 18Ni300 composite material reaches a peak value of 536.5HV; that is, increasing the temperature can accelerate the aging precipitation process, and can accelerate the enrichment of metals, accelerate the nucleation and growth of metals, and improve the hardness of the 18Ni300 composite material; When the holding time gradually increases, the hardness remains basically unchanged before the aging peak appears, but it is greatly improved compared with the hardness of solution treatment. The amplitude modulation decomposition and precipitation of the aging phase occurs in a very short time, and the lattice distortion increases after precipitation; the hardness basically does not change between 1-2 hours at the beginning of aging, but the hardness changes between 2-3 hours, that is, the hardness increases during this time; however, after 2-3 hours, the hardness begins to gradually decrease in the later stage of aging; that is, when the temperature is maintained at a certain temperature, the accumulated heat will produce reversed austenite; after aging treatment at 440℃ / 3h, the hardness of 18Ni300 composite material is the highest, 440℃ is selected as the aging temperature, and 3 hours is the optimal aging time; solution treatment at 800℃ / 1h and aging treatment at 440℃ / 3h are adopted as the optimal heat treatment parameters for solution treatment and aging treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a schematic diagram of the steps of the present invention.

[0018] Figure 2 This is a table diagram of the heat treatment process parameter optimization test of the present invention.

[0019] Figure 3 It is a schematic diagram of the phase transition point of the 18Ni300 alloy of the present invention. DETAILED DESCRIPTION

[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] See also Figure 1-Figure 2 The present invention provides a technical solution: a novel heat treatment process for 18Ni300 martensite, comprising the following steps: S1. Setting a heat treatment method for the 18Ni300 composite material: performing a solid solution treatment and an aging treatment on the 18Ni300 composite material, and achieving heat treatment on the 18Ni300 composite material by combining the solid solution treatment and the aging treatment; S2. Set heat treatment items: set heating temperature and holding time for solution treatment and aging treatment respectively, and set cooling method, including furnace cooling and air cooling; S3. Setting the temperature of heat treatment: There are four temperature levels for the heating temperature of solution treatment and four temperature levels for the heating temperature of aging treatment; S4. Set the duration of heat treatment: the heating duration of solution treatment is set to 1h, and the heating duration of aging treatment includes 1h, 2h, 3h and 4h; S5. Set the cooling method for heat treatment: the cooling method for solution treatment is furnace cooling, and the cooling method for aging treatment is air cooling; S6. Detect the hardness of the 18Ni300 composite material: Detect the hardness of the 18Ni300 composite material through a hardness detection device to obtain the best solution treatment and aging treatment to maximize the hardness of the 18Ni300 composite material.

[0022] In order to set the temperature for solution treatment and to set the holding time, in this embodiment, preferably, the four temperature levels of the solution treatment are set to 750°C, 800°C, 850°C and 900°C, and the corresponding holding times are set to 1h, 1h, 1h and 1h, respectively.

[0023] In order to set the temperature for the aging treatment and to set the holding time, in this embodiment, preferably, the four temperature levels of the aging treatment are set to 400°C, 440°C, 480°C and 520°C, respectively, and the four temperature levels of the holding time are set to 1h, 2h, 3h and 4h, respectively; In order to make the temperature and holding time of aging treatment correspond to each other, 8 temperature groups are set, namely 400℃, 440℃, 480℃, 520℃, 440℃, 440℃, 440℃ and 440℃, and the corresponding holding times are 3h, 3h, 3h, 3h, 1h, 2h, 3h and 4h.

[0024] In order to achieve preheat treatment of the 18Ni300 composite material and set the treatment level of the 18Ni300 composite material, in the present embodiment, preferably, before the heat treatment of the 18Ni300 composite material, the 18Ni300 composite material is first preheated, that is, the 18Ni300 composite material is preheated to 600°C at a heating rate of 200-300°C / h, and the 18Ni300 composite material is preheated and kept warm for 10 minutes, and then heated to a treatment temperature of 750°C at a heating rate of 50°C / h, and kept warm for 1 hour, and then multiple solution treatments are carried out, and the solution treatments are carried out at 750°C, 800°C, 850°C and 900°C respectively.

[0025] In order to realize cooling and lowering treatment of the 18Ni300 composite material after solution treatment, in the present embodiment, preferably, the solution treatment is carried out by furnace cooling, and the furnace cooling is to introduce high-purity Ar gas into the furnace, and the Ar pressure is 60-80MPa; specifically, it is cooled to room temperature rapidly at a cooling rate of 5-10℃ / s, and then the hardness of the 18Ni300 composite material is measured.

[0026] In order to process the temperature of the solution treatment and detect the hardness of the 18Ni300 composite material, in this embodiment, preferably, the hardness parameters of the 18Ni300 composite material after the solution treatment are as follows: The heating temperature is 750℃, the holding time is 1h, and the furnace cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 375HV. The heating temperature is 800℃, the holding time is 1h, and the furnace cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 380.23HV. The heating temperature is 850℃, the holding time is 1h, and the furnace cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 317.7HV. The heating temperature is 900℃, the holding time is 1h, and the furnace cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 301.57HV. The hardness of the samples of 18Ni300 composite materials showed a trend of first increasing and then decreasing, that is, the 18Ni300 composite material obtained a high-strength and tough lath martensite matrix during the solid solution process, which refined the recrystallized grains produced during the solid solution process, forming a good synergistic effect with the solid solution of metal elements, and reached a maximum hardness of 380.23HV at 800℃. However, judging from the change in hardness before and after the solid solution, the overall hardness of the alloy decreased with increasing temperature.

[0027] In order to set different parameter levels for the aging treatment and facilitate multi-stage aging treatment, in this embodiment, preferably, the 18Ni300 composite material is treated again by aging treatment after the solution treatment; The 18Ni300 composite material is firstly preheated, that is, the 18Ni300 composite material is preheated to 300°C at a heating rate of 50-100°C / h, and the 18Ni300 composite material is preheated and kept warm for 10 minutes, and then heated to a treatment temperature of 400°C at a heating rate of 40°C / h, and kept warm for 3 hours, and then subjected to multiple aging treatments, aging treatments are carried out at 440°C, 480°C and 520°C respectively, and at a temperature of 440°C, the holding time is 1h, 2h, 3h and 4h respectively, and at temperatures of 480°C and 520°C, the holding time is 3h.

[0028] In order to realize air cooling treatment of 18Ni300 composite material and facilitate cooling treatment, in this embodiment, preferably, the aging treatment is carried out by air cooling, and the air cooling is to place the 18Ni300 composite material at room temperature for slow cooling; and a fan is used to blow air on the 18Ni300 composite material, so that the 18Ni300 composite material is cooled to room temperature at a cooling rate of 1-3℃ / s, and then the hardness of the 18Ni300 composite material is measured.

[0029] In order to achieve multi-level aging treatment of the 18Ni300 composite material, in this embodiment, preferably, the hardness parameters of the 18Ni300 composite material after aging treatment are as follows: The heating temperature is 400℃, the holding time is 3h, and the air cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 529.27HV. The heating temperature is 440℃, the holding time is 1h, and the air cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 536.17HV. The heating temperature is 440℃, the holding time is 2h, and the air cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 532.07HV. The heating temperature is 440℃, the holding time is 3h, and the air cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 536.5HV. The heating temperature is 440℃, the holding time is 4h, and the air cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 509.63HV. The heating temperature is 480℃, the holding time is 3h, and the air cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 511HV. The heating temperature is 520°C, the holding time is 3h, and air cooling is adopted. The hardness of the treated 18Ni300 composite material is 516.4HV.

[0030] Through the detection and treatment, it is determined that after the 18Ni300 composite material is treated, the hardness of the 18Ni300 composite material is detected. In this embodiment, preferably, the hardness of the 18Ni300 composite material under different aging temperatures first increases and then decreases. When the aging temperature is 440°C, the hardness of the 18Ni300 composite material has a peak value of 536.5HV; that is, increasing the temperature can accelerate the process of aging precipitation, and can accelerate the enrichment of metals, accelerate the nucleation and growth of metals, and improve the hardness of the 18Ni300 composite material; When the holding time gradually increases, the hardness remains basically unchanged before the aging peak appears, but it is greatly improved compared with the hardness of solution treatment. The amplitude modulation decomposition and precipitation of the aging phase occurs in a very short time, and the lattice distortion increases after precipitation; the hardness basically does not change between 1-2 hours at the beginning of aging, but the hardness changes between 2-3 hours, that is, the hardness increases during this time; however, after 2-3 hours, the hardness begins to gradually decrease in the later stage of aging; that is, when the temperature is maintained at a certain temperature, the accumulated heat will produce reversed austenite; after aging treatment at 440℃ / 3h, the hardness of 18Ni300 composite material is the highest, 440℃ is selected as the aging temperature, and 3 hours is the optimal aging time; solution treatment at 800℃ / 1h and aging treatment at 440℃ / 3h are adopted as the optimal heat treatment parameters for solution treatment and aging treatment.

[0031] The working principle and use process of the present invention: Step 1, setting a heat treatment method for the 18Ni300 composite material: performing a solid solution treatment and an aging treatment on the 18Ni300 composite material, and achieving heat treatment on the 18Ni300 composite material by combining the solid solution treatment and the aging treatment; Step 2: Set the heat treatment items: Set the heating temperature and holding time for solution treatment and aging treatment respectively, and set the cooling method, which includes furnace cooling and air cooling; Step 3: Set the temperature of heat treatment: There are four temperature levels for the heating temperature of solution treatment and four temperature levels for the heating temperature of aging treatment; Step 4: Set the duration of heat treatment: the heating duration of solution treatment is set to 1h, and the heating duration of aging treatment includes 1h, 2h, 3h and 4h; Step 5: Set the cooling method for heat treatment: the cooling method for solution treatment is furnace cooling, and the cooling method for aging treatment is air cooling; Step 6: Detect the hardness of the 18Ni300 composite material: Detect the hardness of the 18Ni300 composite material through a hardness detection device, obtain the best solution treatment and aging treatment, so that the hardness of the 18Ni300 composite material reaches the maximum; During the solution treatment, the hardness of the sample of 18Ni300 composite material showed a trend of first increasing and then decreasing, that is, the 18Ni300 composite material obtained a high-strength and tough lath martensite matrix during the solution process, which made the recrystallized grains produced during the solution process refined, forming a good synergistic effect with the solution of metal elements, and reached a maximum hardness of 380.23HV at 800℃. However, from the change of hardness before and after the solution treatment, the overall hardness of the alloy decreased with the increase of temperature. During aging treatment, the hardness under the aging temperature first increases and then decreases. When the aging temperature is 440℃, the hardness of the 18Ni300 composite material reaches a peak value of 536.5HV; that is, increasing the temperature can accelerate the aging precipitation process, and can accelerate the enrichment of metals, accelerate the nucleation and growth of metals, and improve the hardness of the 18Ni300 composite material; When the holding time gradually increases, the hardness remains basically unchanged before the aging peak appears, but it is greatly improved compared with the hardness of solution treatment. The amplitude modulation decomposition and precipitation of the aging phase occurs in a very short time, and the lattice distortion increases after precipitation; the hardness basically does not change between 1-2 hours at the beginning of aging, but the hardness changes between 2-3 hours, that is, the hardness increases during this time; however, after 2-3 hours, the hardness begins to gradually decrease in the later stage of aging; that is, when the temperature is maintained at a certain temperature, the accumulated heat will produce reversed austenite; after aging treatment at 440℃ / 3h, the hardness of 18Ni300 composite material is the highest, 440℃ is selected as the aging temperature, and 3 hours is the optimal aging time; solution treatment at 800℃ / 1h and aging treatment at 440℃ / 3h are adopted as the optimal heat treatment parameters for solution treatment and aging treatment.

[0032] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A novel heat treatment process for 18Ni300 martensite, characterized in that: The following steps are included: S1. Setting a heat treatment method for the 18Ni300 composite material: performing a solid solution treatment and an aging treatment on the 18Ni300 composite material, and achieving heat treatment on the 18Ni300 composite material by combining the solid solution treatment and the aging treatment; S2. Set heat treatment items: set heating temperature and holding time for solution treatment and aging treatment respectively, and set cooling method, including furnace cooling and air cooling; S3. Setting the temperature of heat treatment: There are four temperature levels for the heating temperature of solution treatment and four temperature levels for the heating temperature of aging treatment; S4. Set the duration of heat treatment: the heating duration of solution treatment is set to 1h, and the heating duration of aging treatment includes 1h, 2h, 3h and 4h; S5. Set the cooling method for heat treatment: the cooling method for solution treatment is furnace cooling, and the cooling method for aging treatment is air cooling; S6. Detect the hardness of the 18Ni300 composite material: Detect the hardness of the 18Ni300 composite material through a hardness detection device to obtain the best solution treatment and aging treatment to maximize the hardness of the 18Ni300 composite material.

2. The heat treatment process of a novel 18Ni300 martensite according to claim 1 is characterized in that: The four temperature levels of the solution treatment are set to 750° C., 800° C., 850° C. and 900° C., respectively, and the corresponding holding times are set to 1 h, 1 h, 1 h and 1 h, respectively.

3. The heat treatment process of a novel 18Ni300 martensite according to claim 1 is characterized in that: The four temperature levels of the aging treatment are respectively set to 400° C., 440° C., 480° C. and 520° C., and the four temperature levels of the holding time are respectively set to 1 h, 2 h, 3 h and 4 h; In order to make the temperature and holding time of aging treatment correspond to each other, 8 temperature groups are set, namely 400℃, 440℃, 480℃, 520℃, 440℃, 440℃, 440℃ and 440℃, and the corresponding holding times are 3h, 3h, 3h, 3h, 1h, 2h, 3h and 4h.

4. The novel heat treatment process of 18Ni300 martensite according to claim 1 is characterized in that: Before the heat treatment of the 18Ni300 composite material, the 18Ni300 composite material is preheated, that is, the 18Ni300 composite material is preheated to 600°C at a heating rate of 200-300°C / h, and the 18Ni300 composite material is preheated and kept warm for 10 minutes, and then heated to a treatment temperature of 750°C at a heating rate of 50°C / h, and kept warm for 1 hour, and then multiple solution treatments are carried out, respectively at 750°C, 800°C, 850°C and 900°C.

5. The heat treatment process of a novel 18Ni300 composite material according to claim 1 is characterized in that: The solution treatment is carried out by furnace cooling, wherein high-purity Ar gas is introduced into the furnace, and the Ar pressure is 60-80 MPa; specifically, the furnace is cooled to room temperature at a cooling rate of 5-10°C / s, and then the hardness of the 18Ni300 composite material is measured.

6. The novel heat treatment process of 18Ni300 martensite according to claim 1 is characterized in that: The hardness parameters of the 18Ni300 composite material after the solution treatment are as follows: The heating temperature is 750℃, the holding time is 1h, and the furnace cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 375HV. The heating temperature is 800℃, the holding time is 1h, and the furnace cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 380.23HV. The heating temperature is 850℃, the holding time is 1h, and the furnace cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 317.7HV. The heating temperature is 900℃, the holding time is 1h, and the furnace cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 301.57HV. The hardness of the samples of 18Ni300 composite materials showed a trend of first increasing and then decreasing, that is, the 18Ni300 composite material obtained a high-strength and tough lath martensite matrix during the solid solution process, which refined the recrystallized grains produced during the solid solution process, forming a good synergistic effect with the solid solution of metal elements, and reached a maximum hardness of 380.23HV at 800℃. However, judging from the change in hardness before and after the solid solution, the overall hardness of the alloy decreased with increasing temperature.

7. The novel heat treatment process of 18Ni300 martensite according to claim 1 is characterized in that: After the 18Ni300 composite material is subjected to solution treatment, the 18Ni300 composite material is subjected to aging treatment again; The 18Ni300 composite material is firstly preheated, that is, the 18Ni300 composite material is preheated to 300°C at a heating rate of 50-100°C / h, and the 18Ni300 composite material is preheated and kept warm for 10 minutes, and then heated to a treatment temperature of 400°C at a heating rate of 40°C / h, and kept warm for 3 hours, and then subjected to multiple aging treatments, aging treatments are carried out at 440°C, 480°C and 520°C respectively, and at a temperature of 440°C, the holding time is 1h, 2h, 3h and 4h respectively, and at temperatures of 480°C and 520°C, the holding time is 3h.

8. The novel heat treatment process of 18Ni300 martensite according to claim 1 is characterized in that: The aging treatment is performed by air cooling, wherein the air cooling is to place the 18Ni300 composite material at room temperature for slow cooling; and a fan is used to blow air on the 18Ni300 composite material so that the 18Ni300 composite material is cooled to room temperature at a cooling rate of 1-3°C / s, and then the hardness of the 18Ni300 composite material is measured.

9. The novel heat treatment process of 18Ni300 martensite according to claim 1 is characterized in that: The hardness parameters of the 18Ni300 composite material after aging treatment are as follows: The heating temperature is 400℃, the holding time is 3h, and the air cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 529.27HV. The heating temperature is 440℃, the holding time is 1h, and the air cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 536.17HV. The heating temperature is 440℃, the holding time is 2h, and the air cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 532.07HV. The heating temperature is 440℃, the holding time is 3h, and the air cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 536.5HV. The heating temperature is 440℃, the holding time is 4h, and the air cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 509.63HV. The heating temperature is 480℃, the holding time is 3h, and the air cooling treatment is adopted. The hardness of the treated 18Ni300 composite material is 511HV. The heating temperature is 520°C, the holding time is 3h, and air cooling is adopted. The hardness of the treated 18Ni300 composite material is 516.4HV.

10. A novel heat treatment process for 18Ni300 martensite according to claim 9, characterized in that: The hardness of the 18Ni300 composite material under different aging temperatures first increases and then decreases. When the aging temperature is 440°C, the hardness of the 18Ni300 composite material reaches a peak value of 536.5HV; that is, increasing the temperature can accelerate the aging precipitation process, and can accelerate the enrichment of the metal, accelerate the nucleation and growth of the metal, and improve the hardness of the 18Ni300 composite material; When the holding time gradually increases, the hardness remains basically unchanged before the aging peak appears, but it is greatly improved compared with the hardness of solution treatment. The amplitude modulation decomposition and precipitation of the aging phase occurs in a very short time, and the lattice distortion increases after precipitation; the hardness basically does not change between 1-2 hours at the beginning of aging, but the hardness changes between 2-3 hours, that is, the hardness increases during this time; however, after 2-3 hours, the hardness begins to gradually decrease in the later stage of aging; that is, when the temperature is maintained at a certain temperature, the accumulated heat will produce reversed austenite; after aging treatment at 440℃ / 3h, the hardness of 18Ni300 composite material is the highest, 440℃ is selected as the aging temperature, and 3 hours is the optimal aging time; solution treatment at 800℃ / 1h and aging treatment at 440℃ / 3h are adopted as the optimal heat treatment parameters for solution treatment and aging treatment.