Process for separating iron by mixing and roasting hematite tailings and siderite

Through the mixed roasting iron selection process of hematite tailings and siderite, the problems of carbon emissions and resource waste during separate treatment are solved, the iron recovery rate is improved, and the self-sufficiency of carbon resources is achieved, ensuring the magnetized roasting effect.

CN118957250APending Publication Date: 2024-11-15MCC NORTH (DALIAN) ENG TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411055438.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Problems of excessive carbon emissions and waste of resources when dealing with hematite tailings and siderite alone.

Method used

Hematite tailings and siderite mixed roasting iron selection process, and hematite coarse concentrate and siderite fine powder are obtained through strong magnetic pre-selecting, crushing, grinding and screening, and mixed with sodium carbonate and carbonaceous reducing agent for Reduce and roast, cool down and perform weak magnetic separation to achieve the recovery of iron concentrate.

Benefits of technology

It improves the iron recovery rate, avoids waste of carbon resources and carbon emissions exceeding the standard, ensures the magnetization roasting effect, and achieves self-sufficiency of carbon resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957250A_ABST
    Figure CN118957250A_ABST
Patent Text Reader

Abstract

The invention relates to a hematite tailing and siderite mixed roasting iron separation process. The process comprises the following steps: (1) performing strong magnetic pre-separation on hematite tailings to obtain hematite rough concentrate; (2) siderite is subjected to crushing, ore grinding and screening, and siderite fine powder is obtained; (3) mixing the siderite fine powder and the hematite rough concentrate, adding sodium carbonate and a carbonaceous reducing agent, and feeding into reduction roasting equipment to obtain a reduction roasting product with magnetized mineral particle surfaces; (4) cooling a reduction roasting product; and (5) the cooled reduction roasting product is subjected to low-intensity magnetic separation, and iron ore concentrate is obtained. According to the method, the hematite rough concentrate and the siderite are subjected to mixed roasting, so that the reducing gas CO discharged by the siderite in the roasting process covers a roasting furnace, the generation of oxidizing atmosphere in a furnace tube is avoided, the magnetizing roasting effect is ensured, meanwhile, Fe2O3 in the hematite tailings can be reduced into Fe3O4, and the waste of carbon resources and excessive emission of carbon are avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mineral processing, and in particular to a new process for comprehensive utilization of hematite tailings and siderite. Background Art

[0002] With the rapid growth of steel production, high-quality iron ore resources have gradually dried up, leading to an iron ore supply crisis. It is imperative to develop low-grade iron ore and ensure the supply of iron ore. Siderite resources are very rich, but the iron grade of siderite using traditional beneficiation methods is only 40% to 55% and the recovery rate is 50% to 60%. Hematite tailings are large in volume, fine in fineness, and high in grade, and have a certain recycling value. However, the current conventional hematite tailings recovery is difficult to enrich iron, the cost is high, and the product grade is low and difficult to sell. The magnetization roasting process has attracted attention as a relatively efficient and reasonable technology for processing difficult-to-benefit ores. Magnetization roasting alone generally requires the addition of a large amount of carbonaceous reducing agent, resulting in a large amount of carbon emissions; while magnetization roasting alone for siderite, the reducing gas emitted is not effectively utilized, resulting in a waste of carbon resources. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a mixed roasting and iron separation process of hematite tailings and siderite, so as to solve the problem of excessive carbon emission and waste of resources caused by separate treatment of hematite tailings and siderite.

[0004] To achieve the above object, the present invention adopts the following technical solutions:

[0005] A process for iron separation by mixed roasting of hematite tailings and siderite, comprising the following steps:

[0006] (1) Pre-selecting the hematite tailings by strong magnetic separation to obtain a hematite concentrate;

[0007] (2) crushing, grinding and screening the siderite to obtain siderite fine powder;

[0008] (3) mixing the siderite fine powder and the hematite coarse concentrate, adding sodium carbonate and a carbonaceous reducing agent, and feeding the mixture into a reduction roasting device to obtain a reduction roasting product with magnetized mineral particle surfaces;

[0009] (4) cooling the reduction roasting product;

[0010] (5) The cooled reduction roasting product is subjected to weak magnetic separation to obtain iron concentrate.

[0011] The iron grade of the hematite tailings in step (1) is 10% to 25%, the iron grade of the hematite rough concentrate is 35% to 40%, and the iron grade of the siderite tailings is 40% to 55%.

[0012] The magnetic field strength of the strong magnetic preselection in step (1) is 10000 to 15000 Oersted.

[0013] The crushing equipment in step (2) is one or both of a cone crusher and a jaw crusher, and the grinding equipment is one or more of a ball mill, a high pressure roller mill, and a tower mill.

[0014] The particle size of the siderite fine powder in step (2) is 0.1 to 1 mm.

[0015] The reduction roasting process described in step (3) is as follows: siderite fine powder and hematite coarse concentrate are mixed in a weight ratio of (2 to 2.5):1 to form a mixed ore, 1% to 1.5% of sodium carbonate by weight of the mixed ore is added, 0.5% to 1% of a carbonaceous reducing agent by weight of the mixed ore is added, and reduction roasting is carried out in a reduction roasting equipment, the reduction roasting time is 5 to 30 minutes, and the reduction roasting temperature is 500 to 700°C.

[0016] The reduction roasting equipment in step (3) is a fluidized roasting furnace.

[0017] The roasted product in step (4) is cooled by water quenching.

[0018] The magnetic field strength of the weak magnetic separation in step (5) is 1000 to 3000 Oersteds.

[0019] The iron concentrate obtained by the mixed roasting of hematite tailings and siderite has an iron grade of more than 60% and an iron recovery rate of more than 75%.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The mixed roasting of the hematite rough concentrate and the siderite in the present invention allows the reducing gas CO gas emitted by the siderite during the roasting process to cover the roasting furnace (3FeCO3→Fe3O4+2CO2+CO), thereby avoiding the generation of an oxidizing atmosphere in the furnace tube and ensuring the magnetization roasting effect. Not only can the iron carbonate in the siderite be reduced to magnetic iron, but the Fe2O3 in the hematite tailings can also be reduced to Fe3O4, thereby achieving self-sufficiency in carbon resources and avoiding waste of carbon resources and excessive carbon emissions. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a structural schematic diagram of the present invention. DETAILED DESCRIPTION

[0023] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.

[0024] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and the like are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, features defined as "first", "second", and the like may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means more than two.

[0025] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances.

[0026] like Figure 1 A process for iron separation by mixed roasting of hematite tailings and siderite is carried out in the following steps:

[0027] (1) The hematite tailings are subjected to strong magnetic preselection to obtain a hematite concentrate; the iron grade of the hematite tailings is 10% to 25%; the magnetic field strength of the strong magnetic preselection is 10,000 to 15,000 Oersted. The iron grade of the hematite concentrate is 35% to 40%

[0028] (2) crushing, grinding and screening the siderite to obtain siderite fine powder with a particle size of 0.1 to 1 mm; the crushing equipment is one or both of a cone crusher and a jaw crusher, and the grinding equipment is one or more of a ball mill, a high pressure roller mill and a tower mill;

[0029] (3) Siderite fine powder (FeCO3 iron grade of 40% to 55%) and hematite coarse concentrate (Fe2O3 iron grade of 35% to 40%) are mixed into a mixed ore in a weight ratio of (2 to 2.5):1, and 1% to 1.5% of the weight of the mixed ore is added with sodium carbonate, and 0.5% to 1% of the weight of the mixed ore is added with a carbonaceous reducing agent, and reduction roasting is carried out in a reduction roasting equipment, which is a fluidized roasting furnace. The material can be fully contacted with the reducing gas, the roasting effect is good, and the roasting quality is uniform; the reduction roasting time is 5 to 30 minutes, and the reduction roasting temperature is 500 to 700°C; a reduction roasting product with magnetized mineral particle surface is obtained;

[0030] (4) water quenching the reduction roasting product to prevent the surface magnetite from being excessively oxidized to weakly magnetic hematite, which would affect the reduction roasting effect;

[0031] (5) The cooled reduction roasting product is subjected to weak magnetic separation to obtain iron concentrate. The magnetic field strength of the weak magnetic separation is 1000 to 3000 Oersted.

[0032] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, and these simple modifications all belong to the protection scope of the present invention. It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations. In addition, the various different embodiments of the present invention can also be arbitrarily combined, as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

[0033] In order to make the purpose, technical scheme and technical effect of the present invention clearer, the technical scheme in the embodiment of the present invention is now clearly and completely described. However, the embodiments described below are only part of the embodiments of the present invention, not all of the embodiments. In combination with the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] Example 1

[0035] A process for iron separation by mixed roasting of hematite tailings and siderite, comprising the following steps:

[0036] (1) The hematite tailings are subjected to strong magnetic preselection to obtain a hematite concentrate, with a particle size of 70% below 0.074 mm; the iron grade of the hematite tailings is 12.50%, the strong magnetic separation field strength is 10,000 Oersted, and a hematite concentrate with an iron grade of 35% is obtained.

[0037] (2) The siderite is crushed, ground and screened in a cone crusher, a jaw crusher, a ball mill and a vibrating screen to obtain siderite fine powder of 0.1 to 1 mm.

[0038] (3) Siderite fine powder (FeCO3 iron grade of 50%) and hematite concentrate (Fe2O3 iron grade of 35%) are mixed in a weight ratio of 2:1 to form a mixed ore, 1% of the weight of the mixed ore is added with sodium carbonate, 0.5% of the weight of the mixed ore is added with a carbonaceous reducing agent (lignite), and the mixed ore is placed in a fluidized bed roaster. The reduction roasting time is 15 minutes and the reduction roasting temperature is 550 degrees.

[0039] (4) Water quenching the high temperature roasting product.

[0040] (5) The cooled product was subjected to weak magnetic separation with a magnetic separation field strength of 1500 Oersted to obtain a magnetic concentrate with an iron grade of 60.15% and an iron recovery rate of 78.50%.

[0041] Example 2

[0042] The method is the same as in Example 1, except that:

[0043] (1) The iron grade of the hematite tailings is 15%, and the strong magnetic separation field strength is 12,000 Oersted, and a hematite rough concentrate with an iron grade of 38% is obtained.

[0044] (2) Siderite is processed by high pressure roller mill, tower mill and vibrating screen to obtain narrow grade siderite fine powder of 0.20-0.5 mm.

[0045] (3) Siderite fine powder (FeCO3 iron grade 45%) and hematite concentrate (Fe2O3 iron grade 38%) are mixed in a weight ratio of 2:1 to form a mixed ore, 1.2% of the weight of the mixed ore by sodium carbonate and 0.8% of the weight of the mixed ore by carbonaceous reducing agent (lignite) are added, and the mixed ore is placed in a fluidized bed roasting equipment. The reduction roasting time is 20 minutes and the reduction roasting temperature is 580°C.

[0046] (4) The water-quenched product was subjected to weak magnetic separation with a magnetic separation field strength of 1800 Oersted to obtain a magnetic concentrate with an iron grade of 61.20% and an iron recovery rate of 76.45%.

[0047] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and basic spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A process for iron separation by mixed roasting of hematite tailings and siderite, characterized in that: Follow these steps: (1) Pre-selecting the hematite tailings by strong magnetic separation to obtain a hematite concentrate; (2) crushing, grinding and screening the siderite to obtain siderite fine powder; (3) mixing the siderite fine powder and the hematite coarse concentrate, adding sodium carbonate and a carbonaceous reducing agent, and feeding the mixture into a reduction roasting device to obtain a reduction roasting product with magnetized mineral particle surfaces; (4) cooling the reduction roasting product; (5) The cooled reduction roasting product is subjected to weak magnetic separation to obtain iron concentrate.

2. The iron separation process of hematite tailings and siderite mixed roasting according to claim 1, characterized in that: The iron grade of the hematite tailings in step (1) is 10% to 25%, the iron grade of the hematite rough concentrate is 35% to 40%, and the iron grade of the siderite tailings is 40% to 55%.

3. The iron separation process of hematite tailings and siderite mixed roasting according to claim 1, characterized in that: The magnetic field strength of the strong magnetic preselection in step (1) is 10000 to 15000 Oersted.

4. The iron separation process of hematite tailings and siderite mixed roasting according to claim 1, characterized in that: The crushing equipment in step (2) is one or both of a cone crusher and a jaw crusher, and the grinding equipment is one or more of a ball mill, a high pressure roller mill, and a tower mill.

5. The iron separation process of hematite tailings and siderite mixed roasting according to claim 1, characterized in that: The particle size of the siderite fine powder in step (2) is 0.1 to 1 mm.

6. The iron separation process of hematite tailings and siderite mixed roasting according to claim 1, characterized in that: The reduction roasting process described in step (3) is as follows: siderite fine powder and hematite coarse concentrate are mixed in a weight ratio of (2 to 2.5):1 to form a mixed ore, 1% to 1.5% of sodium carbonate by weight of the mixed ore is added, 0.5% to 1% of a carbonaceous reducing agent by weight of the mixed ore is added, and reduction roasting is carried out in a reduction roasting equipment, the reduction roasting time is 5 to 30 minutes, and the reduction roasting temperature is 500 to 700°C.

7. The iron separation process of hematite tailings and siderite mixed roasting according to claim 1, characterized in that: The reduction roasting equipment in step (3) is a fluidized roasting furnace.

8. The iron separation process of hematite tailings and siderite mixed roasting according to claim 1, characterized in that: The roasted product in step (4) is cooled by water quenching.

9. The iron separation process of hematite tailings and siderite mixed roasting according to claim 1, characterized in that: The magnetic field strength of the weak magnetic separation in step (5) is 1000 to 3000 Oersteds.

10. The iron concentrate obtained by the mixed roasting and iron separation process of hematite tailings and siderite according to claim 1 has an iron grade of more than 60% and an iron recovery rate of more than 75%.

Citation Information

Cited By

  • A magnetized roasting method based on the regulation of autogenous carbon dioxide internal circulation in siderite.

    CN123108286A