Pellet coating method and device for direct reduction
By using uniform mixing and atomizing spraying technology of coating agents such as calcium hydroxide, calcium carbonate or calcium aluminate with water, the oxidized pellet coating system is simplified, and the complex and costly coating system in the prior art is solved. The problem has improved the production efficiency and cost-effectiveness of direct reduction of iron.
Patent Information
- Application Number
- CN202410893230.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-15
AI Technical Summary
In the existing direct reduction iron process, the oxidized pellet coating system is complex and has a large area, which limits production efficiency and cost control, and the coating composition leads to an increase in the later electric furnace smelting costs.
Use calcium hydroxide, calcium carbonate or calcium aluminate to mix evenly with water, spray it onto the surface of raw material pellets through atomization nozzles, simplify the process flow, reduce equipment investment, and achieve accurate coating through PLC control to improve reduction Gas temperature and productivity.
The cladding system is simplified, investment costs are reduced, vertical furnace productivity and reducing gas temperature are improved, energy consumption of electric furnace steelmaking in later stages is reduced, comprehensive costs are reduced, and pellet adhesions are avoided, and production efficiency is improved.
Smart Images

Figure CN118957251A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of direct iron reduction of oxidized pellets, and in particular relates to a method and device for coating oxidized pellets used in producing direct reduced iron by a vertical furnace process before entering a vertical furnace. Background Art
[0002] Since the introduction of gas-based direct reduction ironmaking units into the metallurgical industry in 1978, many direct reduction ironmaking units have been gradually built around the world. Direct reduction ironmaking units do not require large-scale equipment investment like blast furnaces, nor do they require coke. Therefore, they have developed as iron source facilities for ironmaking, mainly in developing countries that produce natural gas. Direct reduced iron can also be directly reduced using H2, and is considered a preferred option for reducing CO2 emissions in steel metallurgy. Direct reduced iron provides a guarantee for the iron source demand for high-quality steel due to its low content of impurities, low ash content, and cleanliness. Furthermore, the development of HBI (hot briquette iron) technology has made it possible to transport direct reduced iron by sea, opening up a global market. Due to the recent increase in steel demand, the demand for the construction of direct reduced iron units is also increasing, and the gas-based direct reduced iron production capacity has reached 134 million tons in 2023. The increase in the construction of direct reduced iron projects has promoted the development of technology in this field, achieving the large-scale vertical furnace, the strengthening of waste heat recovery equipment, the improvement of catalysts for natural gas reforming, and hot pressed blocks.
[0003] The most critical point in the development of direct reduced iron is the improvement of the amount of CO and H2 consumed in the vertical furnace. These improvements have made a great contribution to the improvement of productivity and unit consumption. The consumption of CO and H2 has improved by more than 25% in the past 30 years. This is mainly due to the control of raw material properties, the improvement of solid-gas contact caused by the homogenization of the air flow inside the vertical furnace, and the high temperature of the reducing gas. In the late 1990s, by applying special coating to the raw material pellets, the temperature of the reducing gas was increased to 900℃, and the productivity of the vertical furnace increased by about 10%.
[0004] The coating of raw pellets plays a good role in increasing the temperature of reducing gas in the shaft furnace, preventing the finished product from sticking, and enhancing the reduction rate. However, the coating systems currently used (such as Figure 2 The equipment is relatively complex and large, with a large raw material warehouse (the raw material warehouse has a volume of 30m 3 The above), pulping equipment, intermediate transition bins, spraying devices, etc., also occupy a large area of the system, becoming an important key link in the direct reduction system, and even a limiting link. The existing process directly uses large high-level silos, relies on tank trucks to transport powder materials, and directly transports the powder materials to the material tank through gas. The storage capacity is large, but there is a risk of long-term storage of plate scarring materials, and the subsequent processing is cumbersome. In addition, if Figure 3As shown, in the prior art, the material is added in a simple and rough way of sprinkling, or in a dry powder direct chute diversion mode, poured onto the pellets of the feeding belt, and only the valve opening size is used. The rough sprinkling cannot control the amount of coating agent slurry. How to use a simple and easy-to-control device to replace the existing system requires technical verification. In addition, the main coating agent at present is mainly silicate cement, and the main component of cement is 2CaO·SiO2. The introduction of the acidic element [Si] must introduce more CaO to neutralize it in the later electric furnace smelting and slag making process. Although the amount is relatively small, it virtually increases the cost and energy consumption of slag making (40-50kWh of electricity is consumed per ton of electric furnace slag). Therefore, it is particularly important to develop a more effective way from the perspective of coating agent, process technology and equipment to apply to the preparation of raw material pellets in the existing direct reduction iron process, which can save investment and shield the restrictive factors.
[0005] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0006] In order to solve the technical problem in the prior art that the raw material pellet coating system is relatively complex and occupies a large area, which limits the technical development of direct reduced iron, a pellet coating device and method for direct reduction are provided.
[0007] The first aspect of the present invention provides a coating method for direct reduction pellets, comprising: uniformly mixing a coating agent and water in a mass ratio of 1:1.5-4, and uniformly spraying the mixture onto the surface of the raw material pellets;
[0008] The coating agent is one or more of calcium hydroxide, calcium carbonate, and calcium aluminate;
[0009] The mass percentage of SiO2 in the coating agent is less than 3.0%.
[0010] In some embodiments, the particle size of the coating agent is -325 mesh.
[0011] In some embodiments, 3.5 to 15 liters of coating agent slurry is sprayed per ton of raw material pellets. Insufficient slurry will result in incomplete coating, while excessive slurry will not only cause unnecessary waste, but also cause spillage on the feeding belt, and even increase artificial dust in the feeding system of the vertical furnace top, increasing the amount of top gas purification treatment.
[0012] In some embodiments, the coating agent slurry spraying rate is 0.9-2.7 tons per 1 million tons of direct reduced iron.
[0013] The second aspect of the present invention provides a pellet coating device for direct reduction, including a coating agent pretreatment device, wherein the outlet of the coating agent pretreatment device is connected to an atomizing nozzle, and the outlet of the atomizing nozzle is arranged above a raw material pellet belt.
[0014] In some embodiments, the coating agent pretreatment device includes a coating agent silo, the outlet of the coating agent silo is connected to a slurrying tank via a vibrating feeder, the bottom outlet of the slurrying tank is connected to a circulation pump, the outlet of the circulation pump is connected to a slurry transition tank, and the outlet of the slurry transition tank is connected to an inlet of the atomizing nozzle.
[0015] In some embodiments, a stirring blade is provided in the coating agent silo.
[0016] In some embodiments, a three-way valve is directly provided between the circulation pump outlet and the slurry transition tank inlet, the first interface and the second interface of the three-way valve are respectively connected to the circulation pump outlet and the slurry transition tank inlet, and the third interface of the three-way valve is connected to the air in the pulping tank.
[0017] In some embodiments, a metering pump is provided at the connection between the slurry transition tank and the atomizing nozzle inlet.
[0018] Compared with the prior art, the technical effects achieved by the present invention are as follows:
[0019] (1) The technical solution provided by the present invention can be implemented without changing the basic mechanical structure of the existing direct reduction process, thereby simplifying the process flow and reducing the investment cost. The reduction gas temperature can be increased to above 1050°C, and the productivity of the vertical furnace can be increased by more than 12%. The simplified method and equipment make the coating system no longer a restrictive link of the vertical furnace system.
[0020] (2) The coating agent used in the present application decomposes at high temperature to obtain CaO, and pure CaO has the effect of high temperature resistance, which not only prevents the pellets from sticking and agglomerating after high-temperature reduction, ensuring the smooth production rhythm, but also can increase the temperature of the reduction process gas and improve production efficiency. In addition, the introduction of CaO can reduce the addition of electric furnace steelmaking lime during the subsequent smelting process (if calcium aluminate powder is used, the slag temperature can be reduced and the fluidity can be improved), thereby saving comprehensive costs.
[0021] (3) The storage silo volume in the prior art is 30m 3 Above, the overall height is more than 30 meters, with two 10m in the middle. 3 The device provided in this application eliminates the storage bin and only has one receiving bin (the coating agent bin, 1m 3), 1 pulping tank, 2 small metering pumps, all on the ground level, no steel structure tower is required, so the cost is only less than 40% of the original, compared with the existing process coating system, the investment is 60% less.
[0022] (4) The present invention adopts PLC control to introduce into the DCS interface of the main control room, so as to ensure synchronous control of feeding and coating, achieve accurate addition and fine operation, and improve the efficiency of addition. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic diagram of a pellet coating device and a process flow for direct reduction of the present invention;
[0024] Figure 2 It is a schematic diagram of the structure of the coating system in the prior art;
[0025] Figure 3 It is a photo schematic diagram of a feeding device in the prior art;
[0026] In the figure:
[0027] 1- atomizing nozzle; 2- three-way valve; 3- circulating pump; 4- pulping tank; 4-1 stirring blade; 5- silo for coating agent; 6- vibrating feeder; 7- raw material pellet belt; 8- slurry transition bin; 9 vertical furnace. DETAILED DESCRIPTION
[0028] The technical solution of the present invention is described below by specific embodiments in conjunction with the accompanying drawings. It should be understood that one or more steps mentioned in the present invention do not exclude the existence of other methods and steps before and after the combination step, or other methods and steps can be inserted between these explicitly mentioned steps. It should also be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. Unless otherwise specified, the numbering of each method step is only for the purpose of identifying each method step, and is not intended to limit the order of arrangement of each method or to define the scope of implementation of the present invention. Changes or adjustments in their relative relationships can also be regarded as the scope of implementation of the present invention without substantial changes in the technical content.
[0029] The sources of the raw materials and instruments used in the examples are not particularly limited and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.
[0030] Example 1
[0031] The pellet coating agent is Ca(OH)2, and the slurry is prepared according to the ratio of 1 kg of Ca(OH)2 to 1.5 kg of water.
[0032] like Figure 1As shown, a -325 mesh Ca(OH)2 coating agent is put into a coating agent silo 5, and under the action of a vibrating feeder 6, the Ca(OH)2 coating agent is added to a pulping tank 4, and water 1.5 times the mass of the Ca(OH)2 coating agent is added. The pulping tank 4 is a top electrode with an impeller installed to form a stirring blade 4-1, and the coating agent and water are mixed evenly by the stirring blade 4-1. At the same time, the first valve and the third valve of the three-way valve 2 are opened, and the second valve is closed. A closed loop is formed between the pulping tank 4 and the circulating pump 3, and the circulating pump 3 is turned on. The slurry circulates between the pulping tank 4 and the circulating pump 3, and the duration is 30 minutes, ensure that the slurry is uniform, stable and not stratified, open the third valve of the three-way valve 2, the coating agent slurry enters the slurry transition bin 8, open the outlet switch of the slurry transition bin 8, and the coating agent slurry flows to the atomizing nozzle 1. A metering pump (precise metering plunger pump) is provided at the connection between the atomizing nozzle 1 and the slurry transition bin 8. The amount of the coating agent slurry is measured by the metering pump. Relying on the outlet pressure of the metering pump, the slurry penetrates and evenly coats the surface of the pellets on the raw material pellet belt 7. With the operation of the raw material pellet belt 7, the pellets that are screened after being coated and standing are brought into the vertical furnace 9 on the vertical belt feeding system to ensure the subsequent gas-solid diffusion reduction.
[0033] At least one atomizing nozzle 1 and related pipelines are fixed above the raw material pelletizing belt 7 . Preferably, at least two atomizing nozzles 1 are fixed above the raw material pelletizing belt 7 .
[0034] In one embodiment, the metering pump has a pressure of 1 MPa and a metering rate of -25 L / H per hour.
[0035] A measured volume of 6 liters of coating agent slurry is sprayed per ton of pellets. Based on an annual production scale of 1 million tons of direct reduced iron, 0.9 to 2.7 tons of slurry is required per hour.
[0036] In one embodiment, the direct reduction pellet coating device is introduced into the DCS interface of the main control room using PLC control to ensure synchronous control of feeding and coating, achieve accurate addition and fine operation, and improve the efficiency of addition.
[0037] Since pure Ca(OH)2 reacts as follows at high temperatures of 500-600°C: Ca(OH)2=CaO+H2O, and pure CaO is resistant to high temperatures, when the pellets are properly coated with CaO, the pellets after reduction in the shaft furnace do not participate in the reaction due to the presence of gangue, and the enriched gangue and reduced iron, iron carbide, etc. form a mixture, that is, the furnace bed temperature is increased by reducing "adhesion". Some low-melting point substances will adhere to it, and if not blocked, they will form large agglomerates, blocking the material downstream channel and causing production to be disrupted. The coated pellets help improve production efficiency because the furnace bed permeability is improved. Through the control of raw materials, the improvement of solid-gas contact caused by the homogenization of the airflow inside the shaft furnace, and the high temperature of the reducing gas, it can be increased to 1050°C, and the productivity of the shaft furnace has increased by about 12%. These improvements are achieved without changing the basic mechanical structure of the direct reduction process.
[0038] Example 2
[0039] The calcium aluminate (CaO·Al2O3) coated raw materials are slurried in the ratio of 1 kg of CaO·Al2O3 to 1.5 kg of water to ensure smooth running without sticking in the vertical furnace, which is beneficial to the subsequent electric furnace smelting and slag making.
[0040] Under the condition of ensuring smooth running without sticking in the vertical furnace, 3.5L of slurry is sprayed for each ton of pellets. Since the melting point of CaO·Al2O3 is greater than 1350℃, the coated pellets undergo gas-solid reaction at 1050℃ in the vertical furnace. Calcium aluminate is a cement raw material with fire resistance and the function of improving product strength. It does not affect the quality of the finished product and the metallization rate of direct reduced iron, and at the same time improves the efficiency. The attached calcium aluminate plays a role of fluxing during electric furnace smelting, improves the electric furnace slag making system, and promotes metallurgical effect.
[0041] Example 3
[0042] Calcium aluminate is used to coat the raw material, and pulping is performed in a ratio of 1 kg of calcium aluminate to 4 kg of water.
[0043] In the operation of the 1 million ton shaft furnace, only coated iron ore was fed when the shaft furnace charge was loaded to 642 tons. The coating system was started, with 3 kg of calcium aluminate per ton of iron ore; the concentration of the coating solution was adjusted to about 20%. In two consecutive weeks of operation, 30,445 tons of DRI were produced, and the daily production plan was 2,245-2,700 tons. With 3 kg of calcium aluminate coated per ton of pellets (slurry concentration 20%), the pellet strength was good, the shaft furnace ran smoothly, and the average metallization rate of the finished DRI was controlled at 94%, and the average carbon content was controlled at 3%. Calcium aluminate has a high melting point and is infusible. Coating with calcium aluminate plays a role in coating and preventing adhesion between pellets.
[0044] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.
Claims
1. A method for coating pellets for direct reduction, It is characterized in that include: The coating agent and water are mixed evenly in a mass ratio of 1:1.5-4, and the obtained coating agent slurry is evenly sprayed onto the surface of the raw pellets; The coating agent is one or more of calcium hydroxide, calcium carbonate, and calcium aluminate; The coating agent contains SiO 2 The mass percentage is less than 3.0%.
2. The method for coating pellets for direct reduction according to claim 1, It is characterized in that The particle size of the coating agent is -325 mesh.
3. The method for coating pellets for direct reduction according to claim 1, It is characterized in that 3.5 to 15 liters of coating agent slurry is sprayed per ton of raw pellets.
4. The method for coating pellets for direct reduction according to claim 1, It is characterized in that The spraying rate of the coating agent slurry is 0.9 to 2.7 tons per 1 million tons of direct reduced iron.
5. A pellet coating device for direct reduction, It is characterized in that It comprises a coating agent pretreatment device, the outlet of which is connected to an atomizing nozzle, and the outlet of the atomizing nozzle is arranged above a raw material pellet belt.
6. The pellet coating device for direct reduction according to claim 5, It is characterized in that The coating agent pretreatment device includes a coating agent silo, the coating agent silo outlet is connected to a pulping tank via a vibrating feeder, the pulping tank bottom outlet is connected to a circulation pump, the circulation pump outlet is connected to a slurry transition tank, and the slurry transition tank outlet is connected to the atomizing nozzle inlet.
7. The pellet coating device for direct reduction according to claim 6, It is characterized in that A stirring blade is arranged in the coating agent silo.
8. The pellet coating device for direct reduction according to claim 6, It is characterized in that A three-way valve is directly provided at the circulation pump outlet and the slurry transition bin inlet, the first interface and the second interface of the three-way valve are respectively connected to the circulation pump outlet and the slurry transition bin inlet, and the third interface of the three-way valve is connected to the air in the pulping tank.
9. The pellet coating device for direct reduction according to claim 6, It is characterized in that A metering pump is provided at the connection between the slurry transition bin and the atomizing nozzle inlet.
Citation Information
Cited By
Method for synergistically strengthening direct reduction of pyrite through biochar and calcium hydroxide