Resource utilization method of lithium-containing waste

Through the use of hydrochloric acid leaching and specific extraction agents, combined with multiple pH adjustments, the problem of recycling valuable metals in waste cassettes of lithium-ion batteries is solved, and efficient recycling of lithium, nickel, cobalt, manganese and separation of aluminum are achieved. , avoid the generation of hazardous waste, and improve resource utilization and environmental protection value.

CN118957271AActive Publication Date: 2024-11-15HUNAN BRUNP RECYCLING TECH CO LTD +2
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411051112.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-15
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The prior art has cumbersome steps when recycling lithium-ion batteries and cannot effectively recover other valuable metals other than lithium elements, resulting in waste of resources and environmental pollution.

Method used

Acid leaching is carried out with hydrochloric acid, combined with specific extraction agents (such as TBP, FeCl3 and P507) for extraction and pH adjustment, so as to achieve efficient recycling of lithium, nickel, cobalt, manganese and aluminum, and use acid leaching slag as building materials or cement raw materials , sodium hydroxide is used to perform multiple pH adjustments to achieve metal separation.

Benefits of technology

It realizes efficient recycling of valuable metals in lithium-ion battery waste, avoids the generation of hazardous waste, and improves resource utilization and environmental protection value, and the extractant has excellent separation effect on lithium and aluminum.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957271A_ABST
    Figure CN118957271A_ABST
Patent Text Reader

Abstract

The invention relates to a lithium-containing waste material resource utilization method, which comprises: carrying out acid leaching on a lithium-containing waste material by using hydrochloric acid to obtain acid leaching residue and an acid leaching liquid; extracting the obtained pickle liquor by using an extracting agent to obtain extract liquor and raffinate; the pH value of the obtained raffinate is adjusted at least twice, and aluminum and nickel, cobalt and manganese elements are recycled; carrying out reverse extraction on the obtained extracting solution to obtain a lithium-rich solution; the lithium-rich liquid is used for preparing a lithium product after being subjected to impurity removal. According to the resource utilization method provided by the invention, valuable metal elements in the lithium-containing waste can be efficiently recycled, generation of hazardous waste is avoided, meanwhile, the acid leaching residues can be used as raw materials of building materials and cement, and extremely high economic and environment-friendly values are achieved; in addition, by using the specific extraction agent, efficient separation of Li and Al can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery resource recovery, and relates to a method for resource utilization of battery waste, and in particular to a method for resource utilization of lithium-containing waste. Background Art

[0002] During the production and use of lithium-ion batteries, lithium-containing waste materials containing elements such as lithium, nickel, cobalt and manganese will be generated. If these lithium-containing waste materials are not recycled, it will not only cause a waste of valuable metals, but also cause environmental pollution.

[0003] Taking saggers as an example, saggers are often used as sintering solutions for positive electrode materials of lithium-ion batteries. During the sintering process, lithium sources such as lithium carbonate or lithium hydroxide react fully with precursors containing elements such as nickel, cobalt, and manganese to prepare positive electrode materials. However, in this process, the lithium source will also react with the sagger. Due to the occurrence of side reactions, the saggers are scrapped after a certain number of uses, but the scrapped saggers contain high-grade valuable metals such as lithium, nickel, cobalt, and manganese. Direct scrapping will cause a waste of resources and will also generate higher hazardous waste disposal costs.

[0004] CN109911909A discloses a method for recycling and treating waste saggers in the process of preparing lithium cobalt oxide positive electrode materials, comprising: mixing the waste saggers, acid and additives, performing leaching reaction, and separating to obtain a purified sagger and a leachate; adjusting the pH of the leachate to 2-4, performing solid-liquid separation to obtain solid slag and a separation liquid; adjusting the pH of the separation liquid to 4.5-5.5, performing solid-liquid separation to obtain solid slag and an aluminum-removing liquid; adjusting the pH value of the aluminum-removing liquid, performing solid-liquid separation to obtain a cobalt-containing substance and a cobalt precipitation liquid; adjusting the pH value of the cobalt precipitation liquid, performing solid-liquid separation to obtain a solid slag and a magnesium-removing liquid; adding a precipitant to the magnesium-removing liquid, performing solid-liquid separation to obtain a lithium-containing substance and a lithium-precipitating liquid.

[0005] CN109911946A discloses a method for recycling and treating waste saggers in the process of preparing cobalt-acid lithium battery materials, comprising: mixing the waste saggers, an acid solution and an additive, carrying out a leaching reaction, separating after the reaction to obtain a purified sagger and a leachate; adjusting the pH value of the leachate to separate and obtain solid slag and a separated liquid; adding an aluminum removal agent to the separated liquid, crystallizing, and then separating to obtain solid slag and an aluminum removal liquid; adjusting the pH value of the aluminum removal liquid to separate and obtain cobalt-containing substances and a cobalt precipitation liquid; adding a magnesium removal agent to the cobalt precipitation liquid to separate and obtain solid slag and a magnesium removal liquid; adding a precipitant to the magnesium removal liquid to react, and separating and obtain lithium-containing substances and a lithium precipitation liquid.

[0006] The process steps of the method for recycling waste saggers disclosed in the prior art are relatively complicated, and there is no way to effectively recover other valuable elements besides lithium. Therefore, it is necessary to provide a resource utilization method for lithium-containing waste that can fully recycle and utilize valuable metals in lithium-containing waste. Summary of the invention

[0007] The object of the present invention is to provide a method for resource utilization of lithium-containing waste, which can efficiently recover valuable metal elements in lithium-containing waste and avoid the generation of hazardous waste. At the same time, the acid leaching residue can be used as a raw material for building materials and cement, and has extremely high economic and environmental value. Moreover, the use of the specific extractant of the present invention can also achieve efficient separation of Li and Al.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] The present invention provides a method for resource utilization of lithium-containing waste, and the resource utilization method comprises the following steps:

[0010] (1) using hydrochloric acid to acid-leach the lithium-containing waste material to obtain acid-leaching residue and acid-leaching solution;

[0011] (2) extracting the acid leaching solution obtained in step (1) with an extractant to obtain an extract and a raffinate;

[0012] (3) The pH value of the raffinate obtained in step (2) is adjusted at least twice to recover aluminum and nickel, cobalt and manganese elements;

[0013] (4) The extract obtained in step (2) is stripped to obtain a lithium-rich solution; the lithium-rich solution is used for the preparation of lithium products after impurities are removed;

[0014] Step (3) and step (4) are performed in no particular order;

[0015] The extractant in step (2) includes a first component, a second component, a third component and a diluent; the first component includes TBP (tributyl phosphate) and / or a TBP derivative; the second component includes FeCl3; the third component includes P507 (2-ethylhexyl mono-2-ethylhexyl phosphate) and / or a P507 derivative.

[0016] The lithium-containing waste mentioned in the present invention refers to solid waste containing lithium, nickel, cobalt, manganese and aluminum elements generated during the production and use of lithium-ion batteries. The resource utilization method provided by the present invention can efficiently recover the valuable metal elements in the lithium-containing waste, avoiding the generation of hazardous waste. At the same time, the acid leaching residue can be used as a raw material for building materials and cement, and has extremely high economic and environmental value.

[0017] Moreover, the extractant used in the resource utilization method provided by the present invention has a very good separation effect on Li and Al; acid leaching with hydrochloric acid can achieve a good leaching effect on lithium, nickel, cobalt and manganese under conditions of a relatively low pH value, and the leached residue can be used as a raw material for building materials and cement, thereby achieving efficient separation of lithium and aluminum.

[0018] Preferably, the concentration of the hydrochloric acid used in step (1) is 30-35wt%, for example, it can be 30wt%, 31wt%, 32wt%, 33wt%, 34wt% or 35wt%, but is not limited to the listed values, and the remaining values ​​within the numerical range not listed are also applicable.

[0019] When hydrochloric acid within a concentration range is used in the present invention, good leaching effects of lithium, nickel, cobalt and manganese can be achieved.

[0020] Preferably, the lithium-containing waste in step (1) comprises waste saggers.

[0021] The main materials of saggers include cordierite, mullite and alumina. In the process of using saggers to prepare lithium-ion positive electrode materials, lithium sources such as aluminum hydroxide and lithium carbonate will react with the saggers, resulting in the presence of valuable metals such as nickel, cobalt, manganese, lithium, and aluminum in the waste saggers. Therefore, by recycling the valuable metals in the waste saggers, sustainable utilization of resources can be achieved and the harm of solid waste to the environment can be reduced.

[0022] Preferably, in terms of mass percentage, the content of Li element in the waste sagger is 1.8-2.2wt%, the content of Ni element is 0.15-0.2wt%, the content of Co element is 0.15-0.2wt%, and the content of Mn element is 0.15-0.2wt%.

[0023] In terms of mass percentage, the content of Li element in the waste sagger is 1.8-2.2wt%, for example, it can be 1.8wt%, 1.9wt%, 2wt%, 2.1wt% or 2.2wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0024] In terms of mass percentage, the content of Ni element in the waste sagger is 0.15-0.2wt%, for example, it can be 0.15wt%, 0.16wt%, 0.18wt%, 0.19wt% or 0.2wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0025] In terms of mass percentage, the content of Co element in the waste sagger is 0.15-0.2wt%, for example, it can be 0.15wt%, 0.16wt%, 0.18wt%, 0.19wt% or 0.2wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] In terms of mass percentage, the content of Mn element in the waste sagger is 0.15-0.2wt%, for example, it can be 0.15wt%, 0.16wt%, 0.18wt%, 0.19wt% or 0.2wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] Preferably, the acid leaching temperature in step (1) is 60-90°C, for example, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C or 90°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0028] Preferably, the acid leaching time in step (1) is 1-5 h, for example, 1 h, 2 h, 3 h, 4 h or 5 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0029] Preferably, during the acid leaching, the liquid-to-solid ratio of the lithium-containing waste to water is (2-10) mL:1g; for example, it can be 2 mL:1g, 4 mL:1g, 5 mL:1g, 6 mL:1g, 8 mL:1g or 10 mL:1g, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] Preferably, in terms of mass percentage, the extractant in step (2) comprises 30-50 wt% of the first component, 1-4 wt% of the second component, 20-40 wt% of the third component and the remainder of the diluent.

[0031] Taking the total mass percentage of the first component, the second component, the third component and the diluent as 100wt%, the mass percentage of the first component in the extractant is 30-50wt%, for example, it can be 30wt%, 35wt%, 40wt%, 45wt% or 50wt%, but is not limited to the listed values, and the remaining unlisted values ​​within the numerical range are also applicable.

[0032] Taking the total mass percentage of the first component, the second component, the third component and the diluent as 100wt%, the mass percentage of the second component in the extractant is 1-4wt%, for example, it can be 1wt%, 2wt%, 3wt% or 4wt%, but is not limited to the listed values, and the remaining unlisted values ​​within the numerical range are also applicable.

[0033] Taking the total mass percentage of the first component, the second component, the third component and the diluent as 100wt%, the mass percentage of the third component in the extractant is 20-40wt%, for example, it can be 20wt%, 25wt%, 30wt%, 35wt% or 40wt%, but is not limited to the listed values, and the remaining unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the diluent comprises kerosene.

[0035] Preferably, before the extraction in step (2), the pH value and chloride ion concentration of the acid leaching solution are adjusted.

[0036] The extractant used in the present invention has a stronger extraction effect on hydrogen ions than lithium ions, so the pH value of the acid leaching solution needs to be adjusted, but it is necessary to ensure that the chloride ion concentration in the acid leaching solution is within an appropriate numerical range while adjusting the pH value.

[0037] Preferably, before the extraction in step (2), the pH value of the acid extract is adjusted to 1.5-2.5, for example, 1.5, 1.8, 2, 2.2 or 2.5, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0038] Preferably, before the extraction in step (2), the chloride ion concentration of the acid leaching solution is adjusted to 4.95-7.61 mol / L, for example, 4.95 mol / L, 5 mol / L, 6 mol / L, 7 mol / L or 7.61 mol / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0039] Preferably, before the extraction in step (2), the pH value and chloride ion concentration of the acid leaching solution are adjusted using hydrochloric acid and / or aluminum hydroxide. The present invention does not further limit the concentration of hydrochloric acid herein, as long as the pH value of the acid leaching solution can be adjusted to 1.5-2.5 and the chloride ion concentration can be adjusted to 4.95-7.61 mol / L.

[0040] Further preferably, the aluminum hydroxide comes from adjusting the pH value of the extract at least twice.

[0041] Preferably, the pH value of the raffinate obtained in step (2) is adjusted twice to achieve the recovery of aluminum and nickel, cobalt and manganese elements:

[0042] The raffinate obtained in step (2) is subjected to a first-stage value adjustment and a second-stage value adjustment in sequence, wherein the first-stage value adjustment realizes the recovery of aluminum hydroxide, and the second-stage value adjustment realizes the recovery of nickel, cobalt and manganese hydroxides.

[0043] Preferably, the first stage of adjustment is performed using sodium hydroxide.

[0044] Preferably, the pH value of the first adjustment stage is 4-6, for example, 4, 5 or 6, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0045] Preferably, the temperature of the first adjustment stage is 60-90°C, for example, 60°C, 70°C, 80°C or 90°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0046] Preferably, the adjustment time is 1-5 hours, for example, 1 hour, 2 hours, 3 hours, 4 hours or 5 hours, but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable.

[0047] Under the one-stage adjustment conditions provided by the present invention, the recovery of aluminum hydroxide can be achieved. As a further preferred technical solution, the recovered aluminum hydroxide can be used to adjust the pH value of the acid leaching solution.

[0048] Preferably, the second stage adjustment is performed using sodium hydroxide.

[0049] Preferably, the pH value of the second-stage adjustment is 9-11, for example, 9, 10 or 11, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0050] Preferably, the temperature of the second stage adjustment is 60-90°C, for example, 60°C, 70°C, 80°C or 90°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0051] Preferably, the two-stage adjustment time is 1-5 hours, for example, it can be 1 hour, 2 hours, 3 hours, 4 hours or 5 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0052] Under the conditions of the two-stage adjustment provided by the present invention, the recovery of nickel, cobalt and manganese hydroxide can be achieved.

[0053] The sodium hydroxide used in the first stage value adjustment and the second stage value adjustment of the present invention includes sodium hydroxide solid or sodium hydroxide solution. In order to avoid excessive solvent introduced by the sodium hydroxide solution, the sodium hydroxide used in the first stage value adjustment and the second stage value adjustment is sodium hydroxide solid.

[0054] Preferably, the stripping agent used in the stripping in step (4) comprises water or dilute hydrochloric acid;

[0055] The concentration of hydrogen ions in the dilute hydrochloric acid is below 0.5 mol / L, for example, it can be 0.1 mol / L, 0.2 mol / L, 0.3 mol / L or 0.4 mol / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0056] In the resource utilization method provided by the present invention, the extraction is carried out under acidic conditions. The use of the stripping agent provided by the present invention can ensure that P507 and / or P507 derivatives are not saponified, so the extraction system does not have an obvious extraction effect on nickel, cobalt and manganese, thereby achieving the separation of Li from Ni, Co and Mn.

[0057] As a preferred technical solution of the resource utilization method provided by the present invention, the resource utilization method comprises the following steps:

[0058] (1) The waste sagger is crushed and ground to a particle size of less than 80 mesh, and then acid-leached for 1-5 hours at 60-90° C. using hydrochloric acid with a concentration of 30-35wt% to obtain acid-leached residue and acid-leached liquid;

[0059] In terms of mass percentage, the content of Li element in the waste sagger is 1.8-2.2wt%, the content of Ni element is 0.15-0.2wt%, the content of Co element is 0.15-0.2wt%, and the content of Mn element is 0.15-0.2wt%;

[0060] During the acid leaching, the liquid-to-solid ratio of the waste sagger and water is (2-10) mL:1 g;

[0061] (2) using hydrochloric acid and / or aluminum hydroxide to adjust the pH value of the acid leaching solution to 1.5-2.5, and adjusting the chloride ion concentration to 4.95-7.61 mol / L, and then using an extractant to extract the acid leaching solution obtained in step (1) to obtain an extract and a raffinate;

[0062] In terms of mass percentage, the extractant in step (2) comprises 30-50 wt% of the first component, 1-4 wt% of the second component, 20-40 wt% of the third component and the remainder of the diluent;

[0063] The first component includes TBP and / or TBP derivatives; the second component includes FeCl3; the third component includes P507 and / or P507 derivatives;

[0064] (3) using sodium hydroxide to sequentially perform a first-stage adjustment and a second-stage adjustment on the raffinate obtained in step (2), wherein the first-stage adjustment realizes the recovery of aluminum hydroxide, and the second-stage adjustment realizes the recovery of nickel, cobalt and manganese hydroxides;

[0065] The pH value of the first stage of adjustment is 4-6, the temperature is 60-90°C, and the time is 1-5h;

[0066] The pH value of the second stage adjustment is 9-11, the temperature is 60-90°C, and the time is 1-5h;

[0067] (4) The extract obtained in step (2) is stripped to obtain a lithium-rich solution; after the lithium-rich solution is impurity-removed, sodium carbonate is added to prepare lithium carbonate;

[0068] The stripping agent used in the stripping includes water or dilute hydrochloric acid with a hydrogen ion concentration of less than 0.5 mol / L;

[0069] Step (3) and step (4) are performed in no particular order.

[0070] The crushing and grinding to a particle size of less than 80 meshes refers to crushing and grinding the waste sagger and taking the part passing through an 80-mesh sieve.

[0071] As a preferred technical solution, if the acid leaching solution obtained in step (1) simultaneously satisfies a pH value of 1.5-2.5 and a chloride ion concentration of 4.95-7.61 mol / L, hydrochloric acid and / or aluminum hydroxide may not be used to adjust the acid leaching solution.

[0072] Compared with the prior art, the present invention has the following beneficial effects:

[0073] The resource utilization method provided by the present invention can efficiently recover the valuable metal elements in the lithium-containing waste, avoiding the generation of hazardous waste. At the same time, the acid leaching residue can be used as a raw material for building materials and cement, and has extremely high economic and environmental protection value. Moreover, the extractant used in the resource utilization method provided by the present invention has a very good separation effect on Li and Al. Acid leaching with hydrochloric acid can achieve a good leaching effect on lithium, nickel, cobalt and manganese under the condition of a relatively low pH value, and the leached residue can be used as a raw material for building materials and cement, achieving efficient separation of lithium and aluminum. BRIEF DESCRIPTION OF THE DRAWINGS

[0074] Figure 1 This is a schematic diagram of the process of the resource utilization method provided by the present invention. DETAILED DESCRIPTION

[0075] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0076] The lithium-containing waste in the specific implementation mode of the present invention is a waste sagger that is crushed and ground through an 80-mesh sieve. In terms of mass percentage, the content of Li element in the waste sagger is 2wt%, the content of Ni element is 0.2wt%, the content of Co element is 0.15wt%, and the content of Mn element is 0.15wt%, which mainly exists in the form of LiAlO2 and ternary positive electrode materials. The above-mentioned limitation on the lithium-containing waste is only for the purpose of clearly explaining the technical solution of the present invention, and is not regarded as a further limitation on the resource utilization method of the lithium-containing waste of the present invention.

[0077] Example 1

[0078] This embodiment provides a Figure 1 The resource utilization method of lithium-containing waste shown in the figure comprises the following steps:

[0079] (1) using 31 wt % hydrochloric acid to acid-leach 1000 g of lithium-containing waste at 75° C. for 3 h to obtain acid-leached residue and an acid-leaching solution with a pH value of 6.2;

[0080] During the acid leaching, the liquid-to-solid ratio of the waste sagger and water is 2mL:1g;

[0081] The obtained acid leaching residue is aluminum slag, which can be used as building materials and cement raw materials after simple post-treatment;

[0082] (2) adjusting the pH value of the acid leaching solution to 2 using hydrochloric acid, wherein the adjusted chloride ion concentration is 7.13 mol / L, and then extracting the acid leaching solution obtained in step (1) using an extractant to obtain an extract and a raffinate;

[0083] In terms of mass percentage, the extractant in step (2) comprises 40wt% TBP, 30wt% P507 and 2wt% FeCl3, and the diluent is kerosene;

[0084] (3) using sodium hydroxide to sequentially perform a first-stage value adjustment and a second-stage value adjustment on the raffinate obtained in step (2); after the first-stage value adjustment, solid-liquid separation is performed to recover aluminum hydroxide; and after the second-stage value adjustment, solid-liquid separation is performed to recover nickel, cobalt and manganese hydroxides;

[0085] The pH value of the first stage of adjustment is 4, the temperature is 60°C, and the time is 1h;

[0086] The pH value of the second stage adjustment is 9, the temperature is 60°C, and the time is 1h;

[0087] (4) The extract obtained in step (2) is washed with pure water and stripped to obtain a lithium-rich solution; after the lithium-rich solution is impurity-removed, sodium carbonate is added to prepare lithium carbonate;

[0088] Step (3) and step (4) are performed in no particular order.

[0089] Example 2

[0090] This embodiment provides a Figure 1 The resource utilization method of lithium-containing waste shown in the figure comprises the following steps:

[0091] (1) using 31 wt % hydrochloric acid to acid-leach 1000 g of lithium-containing waste at 75° C. for 3 h to obtain acid-leached residue and an acid-leaching solution with a pH value of 4.4;

[0092] During the acid leaching, the liquid-to-solid ratio of the waste sagger and water is 2mL:1g;

[0093] The obtained acid leaching residue is aluminum slag, which can be used as building materials and cement raw materials after simple post-treatment;

[0094] (2) adjusting the pH value of the acid leaching solution to 2 using hydrochloric acid, wherein the adjusted chloride ion concentration is 7.15 mol / L, and then extracting the acid leaching solution obtained in step (1) using an extractant to obtain an extract and a raffinate;

[0095] In terms of mass percentage, the extractant in step (2) comprises 40wt% TBP, 30wt% P507 and 2wt% FeCl3, and the diluent is kerosene;

[0096] (3) using sodium hydroxide to sequentially perform a first-stage value adjustment and a second-stage value adjustment on the raffinate obtained in step (2); after the first-stage value adjustment, solid-liquid separation is performed to recover aluminum hydroxide; and after the second-stage value adjustment, solid-liquid separation is performed to recover nickel, cobalt and manganese hydroxides;

[0097] The pH value of the first stage of adjustment is 4, the temperature is 60°C, and the time is 1h;

[0098] The pH value of the second stage adjustment is 9, the temperature is 60°C, and the time is 1h;

[0099] (4) The extract obtained in step (2) is washed with pure water and stripped to obtain a lithium-rich solution; after the lithium-rich solution is impurity-removed, sodium carbonate is added to prepare lithium carbonate;

[0100] Step (3) and step (4) are performed in no particular order.

[0101] Example 3

[0102] This embodiment provides a Figure 1 The resource utilization method of lithium-containing waste shown in the figure comprises the following steps:

[0103] (1) using 31 wt % hydrochloric acid to acid-leach 1000 g of lithium-containing waste at 75° C. for 3 h to obtain acid-leached residue and an acid-leaching solution with a pH value of 2.5;

[0104] During the acid leaching, the liquid-to-solid ratio of the waste sagger and water is 2mL:1g;

[0105] The obtained acid leaching residue is aluminum slag, which can be used as building materials and cement raw materials after simple post-treatment;

[0106] (2) The pH value of the acid leaching solution is 2.5, and the chloride ion concentration is 7.02 mol / L. The acid leaching solution obtained in step (1) is extracted with an extractant to obtain an extract and a raffinate;

[0107] In terms of mass percentage, the extractant in step (2) comprises 40wt% TBP, 30wt% P507 and 2wt% FeCl3, and the diluent is kerosene;

[0108] (3) using sodium hydroxide to sequentially perform a first-stage value adjustment and a second-stage value adjustment on the raffinate obtained in step (2); after the first-stage value adjustment, solid-liquid separation is performed to recover aluminum hydroxide; and after the second-stage value adjustment, solid-liquid separation is performed to recover nickel, cobalt and manganese hydroxides;

[0109] The pH value of the first stage of adjustment is 4, the temperature is 60°C, and the time is 1h;

[0110] The pH value of the second stage adjustment is 9, the temperature is 60°C, and the time is 1h;

[0111] (4) The extract obtained in step (2) is washed with pure water and stripped to obtain a lithium-rich solution; after the lithium-rich solution is impurity-removed, sodium carbonate is added to prepare lithium carbonate;

[0112] Step (3) and step (4) are performed in no particular order.

[0113] Example 4

[0114] This embodiment provides a Figure 1 The resource utilization method of lithium-containing waste shown in the figure comprises the following steps:

[0115] (1) using 31 wt % hydrochloric acid to acid-leach 1000 g of lithium-containing waste at 75° C. for 3 h to obtain acid-leached residue and an acid-leaching solution with a pH value of 0.5;

[0116] During the acid leaching, the liquid-to-solid ratio of the waste sagger and water is 2mL:1g;

[0117] The obtained acid leaching residue is aluminum slag, which can be used as building materials and cement raw materials after simple post-treatment;

[0118] (2) using the aluminum hydroxide recovered from the first stage of value adjustment to adjust the pH value of the acid leaching solution to 2, the chloride ion concentration after adjustment is 7.61 mol / L, and using an extractant to extract the acid leaching solution obtained in step (1) to obtain an extract and a raffinate;

[0119] In terms of mass percentage, the extractant in step (2) comprises 40wt% TBP, 30wt% P507 and 2wt% FeCl3, and the diluent is kerosene;

[0120] (3) using sodium hydroxide to sequentially perform a first-stage value adjustment and a second-stage value adjustment on the raffinate obtained in step (2); after the first-stage value adjustment, solid-liquid separation is performed to recover aluminum hydroxide; and after the second-stage value adjustment, solid-liquid separation is performed to recover nickel, cobalt and manganese hydroxides;

[0121] The pH value of the first stage of adjustment is 4, the temperature is 60°C, and the time is 1h;

[0122] The pH value of the second stage adjustment is 9, the temperature is 60°C, and the time is 1h;

[0123] (4) The extract obtained in step (2) is washed with pure water and stripped to obtain a lithium-rich solution; after the lithium-rich solution is impurity-removed, sodium carbonate is added to prepare lithium carbonate;

[0124] Step (3) and step (4) are performed in no particular order.

[0125] Example 5

[0126] This embodiment provides a Figure 1 The resource utilization method of lithium-containing waste shown in the figure comprises the following steps:

[0127] (1) using 31 wt % hydrochloric acid to acid-leach 1000 g of lithium-containing waste at 60° C. for 5 h to obtain acid-leached residue and an acid-leaching solution with a pH value of 6.8;

[0128] During the acid leaching, the liquid-to-solid ratio of the waste sagger and water is 5 mL:1 g;

[0129] The obtained acid leaching residue is aluminum slag, which can be used as building materials and cement raw materials after simple post-treatment;

[0130] (2) adjusting the pH value of the acid leaching solution to 1.5 using hydrochloric acid, wherein the adjusted chloride ion concentration is 4.95 mol / L, and then extracting the acid leaching solution obtained in step (1) using an extractant to obtain an extract and a raffinate;

[0131] In terms of mass percentage, the extractant in step (2) comprises 30 wt % TBP, 40 wt % P507 and 1 wt % FeCl3, and the diluent is kerosene;

[0132] (3) using sodium hydroxide to sequentially perform a first-stage adjustment and a second-stage adjustment on the raffinate obtained in step (2), wherein the first-stage adjustment realizes the recovery of aluminum hydroxide, and the second-stage adjustment realizes the recovery of nickel, cobalt and manganese hydroxides;

[0133] The pH value of the first stage of adjustment is 5, the temperature is 75°C, and the time is 3h;

[0134] The pH value of the second stage adjustment is 10, the temperature is 75°C, and the time is 3h;

[0135] (4) The extract obtained in step (2) is washed with pure water and stripped to obtain a lithium-rich solution; after the lithium-rich solution is impurity-removed, sodium carbonate is added to prepare lithium carbonate;

[0136] Step (3) and step (4) are performed in no particular order.

[0137] Example 6

[0138] This embodiment provides a Figure 1 The resource utilization method of lithium-containing waste shown in the figure comprises the following steps:

[0139] (1) using 31 wt % hydrochloric acid to acid-leach 1000 g of lithium-containing waste at 90° C. for 1 h to obtain acid-leached residue and an acid-leaching solution with a pH value of 7.1;

[0140] During the acid leaching, the liquid-to-solid ratio of the waste sagger and water is 10 mL: 1 g;

[0141] The obtained acid leaching residue is aluminum slag, which can be used as building materials and cement raw materials after simple post-treatment;

[0142] (2) adjusting the pH value of the acid leaching solution to 2.5 using hydrochloric acid, wherein the adjusted chloride ion concentration is 7.57 mol / L, and then extracting the acid leaching solution obtained in step (1) using an extractant to obtain an extract and a raffinate;

[0143] In terms of mass percentage, the extractant in step (2) includes 50wt% TBP, 20wt% P507 and 4wt% FeCl3, and the diluent is kerosene;

[0144] (3) using sodium hydroxide to sequentially perform a first-stage value adjustment and a second-stage value adjustment on the raffinate obtained in step (2); after the first-stage value adjustment, solid-liquid separation is performed to recover aluminum hydroxide; and after the second-stage value adjustment, solid-liquid separation is performed to recover nickel, cobalt and manganese hydroxides;

[0145] The pH value of the first stage of adjustment is 6, the temperature is 90°C, and the time is 5h;

[0146] The pH value of the second stage adjustment is 11, the temperature is 90°C, and the time is 5 hours;

[0147] (4) The extract obtained in step (2) is washed with pure water and stripped to obtain a lithium-rich solution; after the lithium-rich solution is impurity-removed, sodium carbonate is added to prepare lithium carbonate;

[0148] Step (3) and step (4) are performed in no particular order.

[0149] Example 7

[0150] This embodiment provides a method for resource utilization of lithium-containing waste, except that in the extractant described in step (2), the mass percentage of the first component is 20wt%, and the amount of diluent is appropriately adjusted to ensure that the mass percentage of the second component and the third component remains unchanged, the rest is the same as Example 1.

[0151] Example 8

[0152] This embodiment provides a method for resource utilization of lithium-containing waste, except that in the extractant described in step (2), the mass percentage of the first component is 60wt%, and the amount of diluent is appropriately adjusted to ensure that the mass percentage of the second component and the third component remains unchanged, the rest is the same as Example 1.

[0153] Example 9

[0154] This embodiment provides a method for resource utilization of lithium-containing waste, except that in the extractant described in step (2), the mass percentage of the third component is 10wt%, and the amount of diluent is appropriately adjusted to ensure that the mass percentage of the first component and the second component remains unchanged, the rest is the same as Example 1.

[0155] Example 10

[0156] This embodiment provides a method for resource utilization of lithium-containing waste, except that in the extractant described in step (2), the mass percentage of the third component is 50wt%, and the amount of diluent is appropriately adjusted to ensure that the mass percentage of the first component and the second component remains unchanged, the rest is the same as Example 1.

[0157] Comparative Example 1

[0158] This comparative example provides a method for resource utilization of lithium-containing waste, which is the same as Example 1 except that the mass of the third component in the extractant is replaced by the first component.

[0159] Comparative Example 2

[0160] This comparative example provides a method for resource utilization of lithium-containing waste, which is the same as Example 1 except that P507 is replaced by P204.

[0161] Effect Characterization

[0162] In the resource utilization method provided in Examples 1-6, the Li ion concentration, NCM (nickel, cobalt and manganese ion) concentration, Al ion concentration and lithium leaching rate of the acid leaching solution were measured, wherein the concentration of each metal ion was measured using ICP-OES, and the results are shown in Table 1.

[0163] Table 1

[0164] Li(g / L) NCM(g / L) Al(g / L) Lithium leaching rate (%) Example 1 9.0 2.25 34.99 90 Example 2 9.2 2.30 35.77 92 Example 3 9.5 2.38 36.93 95 Example 4 9.6 2.40 37.32 96 Example 5 3.4 0.86 13.37 86 Example 6 1.8 0.46 7.15 92

[0165] In the resource utilization methods provided in the examples and comparative examples, the recovery rates of nickel, cobalt, manganese and lithium were measured, and the results are shown in Table 2.

[0166] Table 2

[0167]

[0168]

[0169] In summary, the resource utilization method provided by the present invention can efficiently recover the valuable metal elements in lithium-containing waste, avoiding the generation of hazardous waste. At the same time, the acid leaching residue can be used as a raw material for building materials and cement, and has extremely high economic and environmental value; moreover, the extractant used in the resource utilization method provided by the present invention has a very good separation effect on Li and Al; acid leaching by hydrochloric acid can achieve a good leaching effect on lithium, nickel, cobalt and manganese under low pH conditions, and the leached residue can be used as a raw material for building materials and cement, achieving efficient separation of lithium and aluminum.

[0170] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A method for recycling lithium-containing waste materials. It is characterized in that The resource utilization method comprises the following steps: (1) using hydrochloric acid to acid-leach the lithium-containing waste material to obtain acid-leaching residue and acid-leaching solution; (2) extracting the acid leaching solution obtained in step (1) with an extractant to obtain an extract and a raffinate; (3) The pH value of the raffinate obtained in step (2) is adjusted at least twice to recover aluminum and nickel, cobalt and manganese elements; (4) The extract obtained in step (2) is stripped to obtain a lithium-rich solution; the lithium-rich solution is used for the preparation of lithium products after impurities are removed; Step (3) and step (4) are performed in no particular order; The extractant in step (2) comprises a first component, a second component, a third component and a diluent; the first component comprises TBP and / or a TBP derivative; the second component comprises FeCl 3 ; The third component includes P507 and / or P507 derivatives.

2. The resource utilization method according to claim 1, It is characterized in that The lithium-containing waste in step (1) includes waste saggers; Preferably, in terms of mass percentage, the content of Li element in the waste sagger is 1.8-2.2wt%, the content of Ni element is 0.15-0.2wt%, the content of Co element is 0.15-0.2wt%, and the content of Mn element is 0.15-0.2wt%.

3. The resource utilization method according to claim 1 or 2, It is characterized in that The acid leaching temperature in step (1) is 60-90° C. Preferably, the acid leaching time in step (1) is 1-5 hours.

4. The resource utilization method according to any one of claims 1 to 3, It is characterized in that In terms of mass percentage, the extractant in step (2) comprises 30-50 wt% of the first component, 1-4 wt% of the second component, 20-40 wt% of the third component and the remainder of the diluent; Preferably, the diluent comprises kerosene.

5. The resource utilization method according to any one of claims 1 to 4, It is characterized in that Before the extraction in step (2), the pH value and chloride ion concentration of the acid leaching solution are adjusted; Preferably, before the extraction in step (2), the pH value of the acid extract is adjusted to 1.5-2.5; Preferably, before the extraction in step (2), the chloride ion concentration of the acid leaching solution is adjusted to 4.95-7.61 mol / L.

6. The resource utilization method according to any one of claims 1 to 5, It is characterized in that The pH value of the raffinate obtained in step (2) is adjusted twice to achieve the recovery of aluminum and nickel, cobalt and manganese elements: The raffinate obtained in step (2) is subjected to a first-stage value adjustment and a second-stage value adjustment in sequence, wherein the first-stage value adjustment realizes the recovery of aluminum hydroxide, and the second-stage value adjustment realizes the recovery of nickel, cobalt and manganese hydroxides.

7. The resource utilization method according to claim 6, It is characterized in that The pH value of the first adjustment stage is 4-6; Preferably, the temperature of the first stage of adjustment is 60-90°C; Preferably, the adjustment period is 1-5 hours.

8. The resource utilization method according to claim 6 or 7, It is characterized in that The pH value of the second stage adjustment is 9-11; Preferably, the temperature of the second stage adjustment is 60-90°C; Preferably, the time for the two-stage adjustment is 1-5 hours.

9. The resource utilization method according to any one of claims 1 to 8, It is characterized in that The stripping agent used in the stripping in step (4) includes water or dilute hydrochloric acid; The concentration of hydrogen ions in the dilute hydrochloric acid is below 0.5 mol / L.

10. The resource utilization method according to claim 1, It is characterized in that The resource utilization method comprises the following steps: (1) The waste sagger is crushed and ground to a particle size of less than 80 mesh, and then acid-leached for 1-5 hours at 60-90° C. using hydrochloric acid with a concentration of 30-35wt% to obtain acid-leached residue and acid-leached liquid; In terms of mass percentage, the content of Li element in the waste sagger is 1.8-2.2wt%, the content of Ni element is 0.15-0.2wt%, the content of Co element is 0.15-0.2wt%, and the content of Mn element is 0.15-0.2wt%; During the acid leaching, the liquid-to-solid ratio of the waste sagger and water is (2-10) mL:1 g; (2) using hydrochloric acid and / or aluminum hydroxide to adjust the pH value of the acid leaching solution to 1.5-2.5, and adjusting the chloride ion concentration to 4.95-7.61 mol / L, and then using an extractant to extract the acid leaching solution obtained in step (1) to obtain an extract and a raffinate; In terms of mass percentage, the extractant in step (2) comprises 30-50 wt% of the first component, 1-4 wt% of the second component, 20-40 wt% of the third component and the remainder of the diluent; The first component includes TBP and / or TBP derivatives; the second component includes FeCl 3 ; The third component includes P507 and / or P507 derivatives; The diluent includes kerosene; (3) using sodium hydroxide to sequentially perform a first-stage adjustment and a second-stage adjustment on the raffinate obtained in step (2), wherein the first-stage adjustment realizes the recovery of aluminum hydroxide, and the second-stage adjustment realizes the recovery of nickel, cobalt and manganese hydroxides; The pH value of the first stage of adjustment is 4-6, the temperature is 60-90°C, and the time is 1-5h; The pH value of the second stage adjustment is 9-11, the temperature is 60-90°C, and the time is 1-5h; (4) The extract obtained in step (2) is stripped to obtain a lithium-rich solution; after the lithium-rich solution is impurity-removed, sodium carbonate is added to prepare lithium carbonate; The stripping agent used in the stripping includes water or dilute hydrochloric acid with a hydrogen ion concentration of less than 0.5 mol / L; Step (3) and step (4) are performed in no particular order.

Citation Information

Patent Citations

  • Method for carrying out recovery treatment on waste saggar in lithium cobaltate positive electrode material preparation process

    CN109911909A

  • Method for carrying out recovery treatment on waste saggar in lithium cobaltate battery material preparation process

    CN109911946A

  • Recycling method of positive electrode powder of waste lithium ion battery

    CN107591584A

  • Method for preparing battery-grade lithium carbonate by extracting lithium from circulating mother liquor for producing aluminum oxide by Bayer process

    CN118001780A

  • KR20220155061A