Preparation method of ultralight high-plasticity magnesium-lithium alloy bar

By adding Zn and Y to the magnesium lithium alloy to form a specific phase, combining hot extrusion and rotary forging, the problems of high energy consumption and mechanical anisotropy in the deformation processing of magnesium lithium alloy are solved, and high-strength and high-plastic magnesium lithium are prepared. The alloy rod material has achieved improved performance and reduced energy consumption of magnesium lithium alloys.

CN118957330APending Publication Date: 2024-11-15NORTHWEST INSTITUTE FOR NONFERROUS METAL RESEARCH
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202411006464.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing magnesium lithium alloys have high energy consumption and mechanical anisotropy problems in deformation processing, which limits the expansion of their engineering applications.

Method used

By adding an appropriate amount of Zn and Y to Mg and Li, the W phase or MgLiZn phase is formed, the grain boundaries are pinned during hot extrusion or cold rotary forging, and the grains are refined, combined with hot extrusion and room temperature rotary forging, so as to improve the The mechanical properties and toughness of magnesium lithium alloys.

Benefits of technology

Under low energy consumption, ultralight high-plastic magnesium-lithium alloy rods with a density of no more than 1.70g/cm2, yield strength of no less than 154MPa, tensile strength of no less than 194MPa, and elongation of no less than 51.5% were prepared, which solved the problem of The problem of insufficient deformation capacity of magnesium alloys at room temperature.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957330A_ABST
    Figure CN118957330A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an ultralight high-plasticity magnesium-lithium alloy bar. The magnesium-lithium alloy bar consists of the following components: 8-14% of Li, 4-8% of Zn, 0.5-2.5% of Y and the balance of Mg. The preparation method comprises the following steps: 1, preparing raw materials; 2, pretreatment; 3, hot extrusion; and 4, performing room-temperature rotary forging. According to the method, Zn and Y are added into the magnesium-lithium alloy to form an Mg3Zn3Y2 phase (W phase) or an MgLiZn phase, the grain boundary is pinned in the hot extrusion or cold rotary swaging process, the growth of recrystallized grains is inhibited, the effect of refining the grains is finally achieved, the mechanical property of the magnesium-lithium alloy is synergistically improved, the mechanical anisotropy existing in the deformed magnesium-lithium alloy is effectively weakened, and the mechanical property of the magnesium-lithium alloy is improved. The density of the ultra-light high-plasticity magnesium-lithium alloy bar is not larger than 1.70 g / cm < 2 >, the yield strength is not lower than 154 MPa, the tensile strength is not lower than 194 MPa, and the ductility is not lower than 51.5%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of magnesium-lithium alloy material processing and manufacturing, and specifically relates to a method for preparing an ultra-light and high-plasticity magnesium-lithium alloy bar. Background Art

[0002] With the rapid development of the aerospace field, the requirements of related equipment for high-performance lightweight metal structural materials are getting higher and higher. Magnesium-lithium alloy has great application potential and prospects in the aerospace field due to its low density, high specific strength, high specific stiffness and excellent functional properties. However, although magnesium-lithium alloy is the lightest metal structural material, its strength and plasticity are not matched and its corrosion resistance is poor. These shortcomings limit the further expansion of its engineering application.

[0003] Alloying is a common method to synergistically improve the performance of magnesium-lithium alloys. Early studies have shown that high-lithium magnesium-lithium alloys have better corrosion resistance because the alloy can form a uniform lithium carbonate film on the surface, and its surface coverage is much higher than that of traditional close-packed hexagonal magnesium alloys. Mg-Li-Zn-Y magnesium-lithium alloys can form a high-density precipitate phase through the composite addition of Zn / Y elements, and the mechanical properties of the alloy can be effectively improved through the coupling effect of the precipitate phase.

[0004] At present, the preparation methods of deformed magnesium-lithium alloys are mainly based on traditional rolling and extrusion. When the magnesium-lithium alloy has a close-packed hexagonal structure, deformation processing is difficult and often requires high-temperature preheating, which increases a lot of energy consumption. In addition, the magnesium-lithium alloy with a close-packed hexagonal structure will also form a strong basal texture during the deformation process. Magnesium-lithium alloys with strong basal texture often have obvious anisotropy of mechanical properties, which in turn affects the subsequent processing and forming of parts.

[0005] Therefore, how to prepare ultra-light and highly plastic magnesium-lithium alloy rods under conditions of low energy consumption is one of the problems that technicians in this field urgently need to solve. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a method for preparing an ultra-light and highly plastic magnesium-lithium alloy rod in view of the deficiencies of the above-mentioned prior art. The method forms a W phase or MgLiZn phase by adding an appropriate amount of Zn and Y to Mg and Li. These phases can pin the grain boundaries during hot extrusion or cold rotary forging, inhibit the growth of recrystallized grains, and finally achieve the effect of grain refinement to obtain an ultra-light and highly plastic magnesium-lithium alloy rod, synergistically improve the mechanical properties of the magnesium-lithium alloy, and effectively weaken the mechanical anisotropy existing in the deformed magnesium-lithium alloy. Combining hot extrusion and room temperature rotary forging, the strength and toughness of the material are synergistically improved, and the problem of insufficient room temperature deformation ability of the magnesium alloy is solved. While obtaining high strength, the fracture elongation of the magnesium-lithium alloy rod is greatly improved, so that the density of the ultra-light and highly plastic magnesium-lithium alloy rod is not more than 1.70g / cm2 , the yield strength is not less than 154MPa, the tensile strength is not less than 194MPa, and the elongation is not less than 51.5%.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing an ultra-light and high-plasticity magnesium-lithium alloy rod, characterized in that the magnesium-lithium alloy rod is composed of the following components by mass fraction: Li 8% to 14%, Zn 4% to 8%, Y 0.5% to 2.5%, and the balance is Mg;

[0008] The magnesium-lithium alloy rod is prepared by the following steps:

[0009] Step 1, preparing raw materials: in a dry or protective atmosphere, cutting magnesium ingots, lithium ingots, zinc ingots and magnesium-yttrium master alloys according to the designed components, and wrapping the lithium ingots with magnesium foil and preserving them in a vacuum to obtain raw materials;

[0010] Step 2, pretreatment: putting the raw material obtained in step 1 into a vacuum induction melting furnace, then closing the furnace cover to evacuate and introduce argon as a protective gas for melting, gradually increasing the power and stirring during the melting process, and then sequentially performing pouring, homogenization treatment and mechanical processing to obtain a pretreated round rod;

[0011] Step 3, hot extrusion: preheating the pretreated round rod obtained in step 2, and then hot extruding and air cooling to obtain a hot extruded round rod;

[0012] Step 4: Room temperature rotary forging: The hot extruded round bar obtained in step 3 is subjected to rotary forging treatment at room temperature to obtain an ultra-light and highly plastic magnesium-lithium alloy bar; the density of the magnesium-lithium alloy bar is not more than 1.70 g / cm 2 , the yield strength is not less than 154MPa, the tensile strength is not less than 194MPa, and the elongation is not less than 51.5%.

[0013] The above-mentioned method for preparing an ultralight and highly plastic magnesium-lithium alloy rod is characterized in that the purity of the magnesium ingot, lithium ingot and zinc ingot in step 1 is greater than 99.9wt.%. The present invention improves the mass purity of the ultralight and highly plastic magnesium-lithium alloy rod by controlling the mass purity of the magnesium ingot, lithium ingot and zinc ingot, prevents the introduction of impurities, and improves the performance of the ultralight and highly plastic magnesium-lithium alloy rod.

[0014] The above-mentioned method for preparing an ultra-light and highly plastic magnesium-lithium alloy bar is characterized in that the smelting power in step 2 is 4kW to 12kW, the time is 20min to 22min, and the temperature of the homogenization treatment is 200℃ to 300℃, and the time is 8h to 12h. The present invention controls the parameters of smelting to fully melt the magnesium ingot, lithium ingot, zinc ingot and magnesium-yttrium master alloy; and controls the parameters of homogenization treatment to avoid significant increase of grain size while homogenizing the structure.

[0015] The above-mentioned method for preparing an ultra-light and highly plastic magnesium-lithium alloy bar is characterized in that the temperatures of the preheating and hot extrusion in step 3 are both 150°C to 350°C, the preheating time is 30min to 60min, the extrusion ratio of the hot extrusion is 16 to 25, and the extrusion speed is 1mm / s to 3mm / s. The present invention improves the fluidity and deformation capacity of the alloy by controlling the preheating parameters, and ensures that the metal is fully deformed by controlling the parameters of the hot extrusion, improves the density of the organization, and at the same time improves the recrystallization ability of the alloy, laying the foundation for subsequent cold deformation.

[0016] The above-mentioned method for preparing an ultra-light and highly plastic magnesium-lithium alloy bar is characterized in that the radial compression amount in step 4 is 0.5 mm to 1 mm, the number of rotary forging passes is 1 to 9 times, and the diameter of the magnesium-lithium alloy bar is 6 mm to 9 mm. The present invention introduces a large number of dislocations by regulating the parameters of rotary forging, and effectively refines the grains, thereby synergistically improving the strength and toughness of the alloy.

[0017] Compared with the prior art, the present invention has the following advantages:

[0018] 1. The present invention adds an appropriate amount of Zn and Y to the magnesium-lithium alloy to form a W phase or a MgLiZn phase. These phases can pin the grain boundary during hot extrusion or cold rotary forging, inhibit the growth of recrystallized grains, and finally achieve the effect of grain refinement to obtain an ultra-light and high-plasticity magnesium-lithium alloy bar, synergistically improve the mechanical properties of the magnesium-lithium alloy, and effectively weaken the mechanical anisotropy existing in the deformed magnesium-lithium alloy. Combining hot extrusion and room temperature rotary forging, the strength and toughness of the material are synergistically improved, and the problem of insufficient room temperature deformation ability of the magnesium alloy is solved. While obtaining high strength, the fracture elongation of the magnesium-lithium alloy bar is greatly improved, so that the density of the ultra-light and high-plasticity magnesium-lithium alloy bar is not more than 1.70g / cm 2 , the yield strength is not less than 154MPa, the tensile strength is not less than 194MPa, and the elongation is not less than 51.5%.

[0019] 2. The present invention uses magnesium ingots, lithium ingots, zinc ingots and magnesium-yttrium master alloys as raw materials, and reduces the introduction of impurity elements by taking materials in a dry or protective atmosphere environment. By controlling the smelting parameters, the magnesium ingots, lithium ingots, zinc ingots and magnesium-yttrium master alloys are fully melted; by controlling the parameters of the homogenization treatment, the significant increase of the grains is avoided while the structure is homogenized.

[0020] 3. The present invention adopts a combination of hot extrusion and cold rotary forging deformation processes to prepare magnesium-lithium alloy rods. The coarse primary phase in the magnesium-lithium alloy is broken up through the composite deformation process, and a large amount of nanophase precipitation is induced at the same time, so that the multi-scale precipitated phases are evenly distributed in the matrix. The final rod has uniform composition, fine grains, and the second phase of the material is easy to control.

[0021] 4. The present invention reduces the energy consumption requirement for preheating treatment during deformation processing. The extrusion and rotary forging equipment used are simple, the processing and preparation process is simple and flexible, and has universal applicability. It is suitable for precipitation phase strengthened magnesium-lithium alloys with α-Mg phase as the matrix, β-Li phase as the matrix, or (α-Mg+β-Li) dual phase as the matrix.

[0022] 5. The present invention has the advantages of short process, low energy consumption and simple process. The size and distribution of the precipitated phase are regulated by a composite process, so that the strength and plasticity of the prepared magnesium-lithium alloy rod are synergistically improved.

[0023] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 1 is a metallographic image of the pretreated round rod obtained in step 2 of Example 1 of the present invention.

[0025] Figure 2 This is a SEM image of the hot extruded round rod obtained in step 3 of Example 1 of the present invention.

[0026] Figure 3 This is a SEM image of the tensile fracture of the magnesium-lithium alloy rod obtained in step 4 of Example 1 of the present invention.

[0027] Figure 4 This is the tensile mechanical property curve of the magnesium-lithium alloy rod obtained in step 4 of Example 1 of the present invention. DETAILED DESCRIPTION

[0028] Example 1

[0029] This embodiment includes the following steps:

[0030] Step 1, preparing raw materials: in a dry or protective atmosphere, cutting magnesium ingots, lithium ingots, zinc ingots and magnesium-yttrium master alloys of required mass according to the designed composition, and wrapping the lithium ingot with magnesium foil and preserving it in a vacuum to obtain raw materials;

[0031] Step 2, pretreatment: the raw materials obtained in step 1 are placed in a vacuum induction melting furnace according to the melting point and size, the furnace cover is closed to evacuate and argon is introduced as a protective gas, and then the power of the vacuum induction melting furnace is increased to 4kW and kept warm for 5 minutes, and then the power is adjusted to 6kW and kept warm for 5 minutes. After the magnesium ingot is completely melted, the power is adjusted to 8kW and kept warm for 8 minutes, and finally the power is increased to 12kW and the stirring function is turned on to mix the metal solution evenly. After standing for 2 minutes, it is poured into a graphite mold with a diameter of 105 mm and a length of 300 mm to form, and then subjected to homogenization annealing and machining at a temperature of 300°C for 8 hours to obtain a pretreated round rod with a diameter of 48 mm;

[0032] Step 3, hot extrusion: put the pretreated round rod obtained in step 2 into a box-type resistance furnace and heat it to 300°C and preheat it for 30 minutes, then use a die with a diameter of 12 mm, an extrusion ratio of 16:1, an extrusion speed of 3 mm / s, and an extrusion temperature of 300°C for extrusion forming, and cool it to room temperature in air to obtain a hot extruded round rod;

[0033] Step 4, room temperature rotary forging: The hot extruded round bar obtained in step 3 is subjected to 4 rotary forging processes at room temperature with a radial compression of no more than 1 mm, the first radial compression is 1 mm, the second radial compression is 1 mm, the third radial compression is 0.9 mm, and the fourth radial compression is 0.6 mm, to obtain an ultra-light and high-plasticity Mg-10.3Li-5.8Zn-1.67Y magnesium-lithium alloy bar with a diameter of 8.5 mm.

[0034] After testing, the axis direction of the magnesium-lithium alloy rod prepared in this embodiment is parallel to the rotary forging direction. The prepared specimens with a standard length of 46 mm and a gauge section diameter of 3 mm are tested for yield strength, tensile strength and elongation, and the strain rate is 1×10 -3 s -1 The yield strength and tensile strength of the magnesium-lithium alloy rod prepared in this embodiment are 160 MPa and 203 MPa respectively, and the elongation is 56%.

[0035] Figure 1 is the metallographic image of the pretreated round rod obtained in step 2 of this embodiment. Figure 1 It can be seen that the matrix of the pretreated round rod is mainly β-Li phase, the black eutectic phase (W phase) is distributed along the grain boundaries, and a large number of fine particle phases (MgLiZn phase) are dispersed inside the grains.

[0036] Figure 2 is a SEM image of the hot extruded round rod obtained in step 3 of this embodiment. Figure 2 It can be seen that the structure of the magnesium-lithium alloy rod is refined after extrusion deformation, and the coarse W phase becomes finer and more dispersed after being broken.

[0037] Figure 3 is a SEM image of the tensile fracture of the magnesium-lithium alloy rod obtained in step 4 of this embodiment. Figure 3 It can be seen that the rod fracture is a ductile fracture. During the fracture process, the tensile specimen undergoes obvious necking, and the fracture surface is mainly composed of dimples, which is an obvious ductile fracture feature.

[0038] Figure 4 is the tensile mechanical property curve of the magnesium-lithium alloy rod obtained in step 4 of this embodiment. Figure 4It can be seen that the yield and tensile strengths of the rod are 160MPa and 203MPa respectively, and the elongation is 56%.

[0039] Example 2

[0040] This embodiment includes the following steps:

[0041] Step 1, preparing raw materials: in a dry or protective atmosphere, cutting magnesium ingots, lithium ingots, zinc ingots and magnesium-yttrium master alloys of required mass according to the designed composition, and wrapping the lithium ingot with magnesium foil and preserving it in a vacuum to obtain raw materials;

[0042] Step 2, pretreatment: the raw materials obtained in step 1 are placed in a vacuum induction melting furnace according to the melting point and size, the furnace cover is closed to evacuate and argon is introduced as a protective gas, and then the power of the vacuum induction melting furnace is increased to 4kW and kept warm for 5 minutes, and then the power is adjusted to 6kW and kept warm for 5 minutes. After the magnesium ingot is completely melted, the power is adjusted to 8kW and kept warm for 10 minutes. Finally, the power is increased to 10kW and the stirring function is turned on to mix the metal solution evenly. After standing for 2 minutes, it is poured into a graphite mold with a diameter of 105 mm and a length of 300 mm to form, and then subjected to homogenization annealing and machining at a temperature of 300°C for 8 hours to obtain a pretreated round rod with a diameter of 50 mm;

[0043] Step 3, hot extrusion: put the pretreated round rod obtained in step 2 into a box-type resistance furnace and heat it to 150°C and preheat it for 60 minutes, then use a die with a diameter of 10 mm, an extrusion ratio of 25:1, an extrusion speed of 1 mm / s, and an extrusion temperature of 150°C to extrude it, and cool it to room temperature in air to obtain a hot extruded round rod;

[0044] Step 4, room temperature rotary forging: The hot extruded round bar obtained in step 3 is subjected to three passes of rotary forging at room temperature with a radial compression of no more than 1 mm, the first pass radial compression is 1 mm, the second pass radial compression is 1 mm, and the third pass radial compression is 1 mm, to obtain an ultra-light and high-plastic Mg-8.5Li-6.2Zn-1.55Y magnesium-lithium alloy bar with a diameter of 7 mm.

[0045] After testing, the axis direction of the magnesium-lithium alloy rod prepared in this embodiment is parallel to the rotary forging direction. The prepared specimens with a standard length of 46 mm and a gauge section diameter of 3 mm are tested for yield strength, tensile strength and elongation, and the strain rate is 1×10 -3 s -1 The yield strength and tensile strength of the magnesium-lithium alloy rod prepared in this embodiment are 197 MPa and 256 MPa respectively, and the elongation is 51.5%.

[0046] Example 3

[0047] This embodiment includes the following steps:

[0048] Step 1, preparing raw materials: in a dry or protective atmosphere, cutting magnesium ingots, lithium ingots, zinc ingots and magnesium-yttrium master alloys of required mass according to the designed composition, and wrapping the lithium ingot with magnesium foil and preserving it in a vacuum to obtain raw materials;

[0049] Step 2, pretreatment: the raw materials obtained in step 1 are placed in a vacuum induction melting furnace according to the melting point and size, the furnace cover is closed to evacuate and argon is introduced as a protective gas, and then the power of the vacuum induction melting furnace is increased to 4kW and kept warm for 5 minutes, and then the power is adjusted to 6kW and kept warm for 5 minutes. After the magnesium ingot is completely melted, the power is adjusted to 8kW and kept warm for 10 minutes. Finally, the power is increased to 10kW and the stirring function is turned on to mix the metal solution evenly. After standing for 2 minutes, it is poured into a graphite mold with a diameter of 105 mm and a length of 300 mm to form, and then subjected to homogenization annealing and machining at a temperature of 200°C for 12 hours to obtain a pretreated round rod with a diameter of 50 mm;

[0050] Step 3, hot extrusion: put the pretreated round rod obtained in step 2 into a box-type resistance furnace and heat it to 350°C and preheat it for 30 minutes, then use a die with a diameter of 10 mm, an extrusion ratio of 25:1, an extrusion speed of 2 mm / s, and an extrusion temperature of 350°C to extrude it, and cool it to room temperature in air to obtain a hot extruded round rod;

[0051] Step 4: Room temperature rotary forging: The hot extruded round bar obtained in step 3 is subjected to rotary forging treatment at room temperature with a radial compression of no more than 1 mm, and the first radial compression is 1 mm, to obtain an ultra-light and high-plasticity Mg-14Li-4Zn-2.5Y magnesium-lithium alloy bar with a diameter of 9 mm.

[0052] After testing, the axis direction of the magnesium-lithium alloy rod prepared in this embodiment is parallel to the rotary forging direction. The prepared specimens with a standard length of 46 mm and a gauge section diameter of 3 mm are tested for yield strength, tensile strength and elongation, and the strain rate is 1×10 -3 s -1 The yield strength and tensile strength of the magnesium-lithium alloy rod prepared in this embodiment are 154 MPa and 194 MPa respectively, and the elongation is 59%.

[0053] Example 4

[0054] This embodiment includes the following steps:

[0055] Step 1, preparing raw materials: in a dry or protective atmosphere, cutting magnesium ingots, lithium ingots, zinc ingots and magnesium-yttrium master alloys of required mass according to the designed composition, and wrapping the lithium ingot with magnesium foil and preserving it in a vacuum to obtain raw materials;

[0056] Step 2, pretreatment: the raw materials obtained in step 1 are placed in a vacuum induction melting furnace according to the melting point and size, the furnace cover is closed to evacuate and argon is introduced as a protective gas, and then the power of the vacuum induction melting furnace is increased to 4kW and kept warm for 5 minutes, and then the power is adjusted to 6kW and kept warm for 5 minutes. After the magnesium ingot is completely melted, the power is adjusted to 8kW and kept warm for 10 minutes, and finally the power is increased to 10kW and the stirring function is turned on to mix the metal solution evenly. After standing for 2 minutes, it is poured into a graphite mold with a diameter of 105 mm and a length of 300 mm to form, and then subjected to homogenization annealing and machining at a temperature of 250°C for 10 hours to obtain a pretreated round rod with a diameter of 49 mm;

[0057] Step 3, hot extrusion: put the pretreated round rod obtained in step 2 into a box-type resistance furnace and heat it to 300°C and preheat it for 40 minutes, then use a die with a diameter of 12 mm, an extrusion ratio of 17:1, an extrusion speed of 1 mm / s, and an extrusion temperature of 300°C for extrusion forming, and cool it to room temperature in air to obtain a hot extruded round rod;

[0058] Step 4, room temperature rotary forging: The hot extruded round bar obtained in step 3 is subjected to 9 passes of rotary forging at room temperature with a radial compression of no more than 1 mm, the first pass of radial compression is 1 mm, and the subsequent eight passes of radial compression are 0.5 mm, to obtain an ultra-light and high-plastic Mg-12.2Li-8Zn-0.5Y magnesium-lithium alloy bar with a diameter of 6 mm.

[0059] After testing, the axis direction of the magnesium-lithium alloy rod prepared in this embodiment is parallel to the rotary forging direction. The prepared specimens with a standard length of 46 mm and a gauge section diameter of 3 mm are tested for yield strength, tensile strength and elongation, and the strain rate is 1×10 -3 s -1 The yield strength and tensile strength of the magnesium-lithium alloy rod prepared in this embodiment are 176 MPa and 225 MPa respectively, and the elongation is 53%.

[0060] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing an ultra-light and highly plastic magnesium-lithium alloy rod, characterized in that: The magnesium-lithium alloy rod is composed of the following components by mass fraction: Li 8% to 14%, Zn 4% to 8%, Y 0.5% to 2.5%, and the balance is Mg; The magnesium-lithium alloy rod is prepared by the following steps: Step 1, preparing raw materials: in a dry or protective atmosphere, cutting magnesium ingots, lithium ingots, zinc ingots and magnesium-yttrium master alloys according to the designed components, and wrapping the lithium ingots with magnesium foil and preserving them in a vacuum to obtain raw materials; Step 2, pretreatment: putting the raw material obtained in step 1 into a vacuum induction melting furnace, then closing the furnace cover to evacuate and introduce argon as a protective gas for melting, gradually increasing the power and stirring during the melting process, and then sequentially performing pouring, homogenization treatment and mechanical processing to obtain a pretreated round rod; Step 3, hot extrusion: preheating the pretreated round rod obtained in step 2, and then hot extruding and air cooling to obtain a hot extruded round rod; Step 4: Room temperature rotary forging: The hot extruded round bar obtained in step 3 is subjected to rotary forging treatment at room temperature to obtain an ultra-light and highly plastic magnesium-lithium alloy bar; the density of the magnesium-lithium alloy bar is not more than 1.70 g / cm 2 , the yield strength is not less than 154MPa, the tensile strength is not less than 194MPa, and the elongation is not less than 51.5%.

2. The method for preparing an ultra-light and highly plastic magnesium-lithium alloy rod according to claim 1, characterized in that: The purity of the magnesium ingot, lithium ingot and zinc ingot in step 1 is greater than 99.9wt.%.

3. The method for preparing an ultra-light and highly plastic magnesium-lithium alloy rod according to claim 1, characterized in that: The smelting power in step 2 is 4 kW to 12 kW, the time is 20 min to 22 min, the temperature of the homogenization treatment is 200° C. to 300° C., and the time is 8 h to 12 h.

4. The method for preparing an ultra-light and highly plastic magnesium-lithium alloy rod according to claim 1, characterized in that: The temperatures of the preheating and hot extrusion in step 3 are both 150° C. to 350° C., the preheating time is 30 min to 60 min, the extrusion ratio of the hot extrusion is 16 to 25, and the extrusion speed is 1 mm / s to 3 mm / s.

5. The method for preparing an ultra-light and highly plastic magnesium-lithium alloy rod according to claim 1, characterized in that: The radial compression amount in step 4 is 0.5 mm to 1 mm, the number of rotary forging passes is 1 to 9 times, and the diameter of the magnesium-lithium alloy rod is 6 mm to 9 mm.

Citation Information

Cited By

  • Lightweight high-strength plastic Mg-Li-Zn-Gd alloy bar and preparation method thereof

    CN119506626A

  • Mg-Y-La alloy and preparation method thereof

    CN119710409A

  • Method for improving performance of double-phase magnesium-lithium alloy through extrusion deformation

    CN120099438A

  • Room-temperature rotary swaging preparation method of high-strength and high-modulus magnesium-lithium-based composite material

    CN120738530A

  • Ultralight high-performance flame-retardant magnesium-lithium alloy bar and preparation method thereof

    CN120818711A