Beryllium-titanium alloy and preparation method thereof
Through vacuum suspension smelting method and electromagnetic field technology, the problems of high impurity content and poor mechanical properties in the preparation of beryllium titanium alloy are solved, and the beryllium titanium alloy with high purity, no pore defects and excellent mechanical properties are achieved, which improves compatibility with stainless steel , meets the performance requirements of the nuclear reactor enclosure layer material.
Patent Information
- Application Number
- CN202411132719.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing beryllium titanium alloy preparation methods have problems such as high impurity content, low sintering densification degree and poor mechanical properties, which are difficult to meet the performance requirements of the nuclear reactor cladding material.
Vacuum suspension smelting method is used to generate the interaction between induced eddy current and magnetic force lines through the electromagnetic field, so that beryllium sheets and titanium particles are suspended or quasi-suspended, avoid crucible contamination and pore defects, improve tissue uniformity and purity, and cool in the copper crucible. forming.
The low impurity content, high sintering densification degree and excellent mechanical properties of beryllium titanium alloy are achieved, the compatibility with stainless steel is improved, and the performance requirements of the nuclear reactor cladding material is met.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of beryllium alloy materials, and in particular relates to a beryllium-titanium alloy and a preparation method thereof. Background Art
[0002] Metal beryllium is a brittle material. The room temperature fracture toughness of pure beryllium is 10MPa.m 1 / 2 The room temperature elongation is only about 3%. Therefore, in view of the brittleness of pure beryllium, its brittleness is improved by alloying and other methods, thereby obtaining Be alloys with better performance. 12 Ti is a beryllium-rich intermetallic compound. As a nuclear reactor jacket material, it has a neutron multiplication capability and tritium multiplication ratio comparable to that of metallic beryllium. It is expected to become a new ITER neutron multiplication material. Compared with metallic beryllium, its melting point is about 300°C higher, and it has better high-temperature stability, high-temperature oxidation resistance, low expansion coefficient and strong corrosion resistance. In addition, Be 12 Ti has fewer irradiation defects under high helium content irradiation, releases tritium faster, stores less tritium at high temperatures, can achieve neutron multiplication capability and tritium proliferation ratio comparable to pure metallic Be, and has better compatibility with stainless steel in the cladding.
[0003] At present, conventional forming processes of beryllium titanium alloy include powder metallurgy (hot isostatic pressing or plasma sintering), hot extrusion and melt casting, etc. The traditional process methods have the characteristics of poor uniformity of alloy structure, high impurity content, low purity, low degree of component densification and poor mechanical properties. For example, the Chinese patent with publication number CN104630524A and invention name of method for preparing beryllium titanium alloy by spark plasma sintering mainly adopts spark plasma sintering process to prepare beryllium titanium alloy, but the impurity content is high, the degree of sintering densification is low, beryllium titanium alloy is prone to pore defects, and poor mechanical properties and other deficiencies or defects. Summary of the invention
[0004] In view of this, one of the objects of the present invention is to provide a method for preparing a beryllium-titanium alloy. The beryllium-titanium alloy prepared by the preparation method has the characteristics of low impurity content, high sintering densification degree, excellent mechanical properties, etc., meets the performance requirements of nuclear reactor cladding layer materials, and improves the compatibility of nuclear reactor cladding layer materials with stainless steel.
[0005] One of the objectives of the present invention is to provide a beryllium-titanium alloy.
[0006] In order to achieve one of the above purposes, the present invention adopts the following technical solutions:
[0007] A method for preparing a beryllium-titanium alloy, the method comprising:
[0008] Step S1, fixing a copper crucible with beryllium sheets and titanium particles in a smelting furnace, water cooling for 3 to 5 minutes and then evacuating, and then continuously filling the smelting furnace with argon until the vacuum pressure in the smelting furnace is -70 to -50 Pa, heating up to 1000 to 1600° C. at a heating rate of 30 to 60° C. / min, and vacuum suspension smelting for 15 to 30 minutes to obtain a suspension smelting liquid;
[0009] In the step S1, the mass percentages of the beryllium sheets and the titanium particles are 70-89wt% and 11-30wt% respectively;
[0010] Step S2, cooling the suspension smelting liquid to a temperature of 100 to 300° C. at a cooling rate of 30 to 40° C. / min, cooling the smelted liquid to form the product, and then performing surface polishing.
[0011] Furthermore, in step S1, the purity of the beryllium sheet is 99.99%; the purity of the titanium particles is 99.999%.
[0012] Furthermore, in step S1, the vacuum degree in the evacuated smelting furnace is 3 to 7×10 -3 Pa;
[0013] The vacuum suspension smelting is carried out at a temperature of 1100 to 1500° C. and for a time of 18 to 27 minutes.
[0014] Furthermore, in the step S1, the vacuum degree in the evacuated smelting furnace is 4.4-5.5×10 - 3 Pa;
[0015] The vacuum suspension smelting is carried out at a temperature of 1200 to 1400° C. and for a time of 20 to 24 minutes.
[0016] Furthermore, in the step S1, the heating rate is 35-55°C / min.
[0017] Furthermore, in the step S1, the heating rate is 40-50°C / min.
[0018] Furthermore, in the step S2, the cooling molding temperature is 150-250°C, and the cooling molding time is 30-50 minutes.
[0019] In order to achieve the second objective above, the present invention adopts the following technical solution:
[0020] A beryllium-titanium alloy is prepared by the above-mentioned preparation method.
[0021] Furthermore, at -50 to 350°C, the longitudinal linear expansion coefficient of the beryllium-titanium alloy is 11.09×10 -6 / ℃~14.09×10 -6 / ℃, the transverse linear expansion coefficient is 10.39×10 -6 / ℃~13.16×10 -6 / ℃.
[0022] In summary, the solution proposed by the present invention has the following technical effects:
[0023] The present invention uses the induced eddy current (right-hand rule) generated by the electromagnetic field in the beryllium sheets and titanium particles, and utilizes the thermal effect of the induced eddy current to achieve the smelting of the beryllium sheets and titanium particles. The present invention utilizes the interaction between the eddy current and the magnetic force lines to generate an electromagnetic force (left-hand rule) perpendicular to both the eddy current and the magnetic force lines, thereby forming a suspension effect, so that the beryllium sheets and titanium particles to be melted are in a suspended or quasi-suspended state, achieving suspension smelting without sticking to the crucible, avoiding the contamination of the crucible material to the metal solution under high temperature conditions, reducing the impurity content, and directly cooling and forming in the copper crucible. The invention avoids the generation of pore defects through the casting process; the microstructure of beryllium titanium is homogenized during the smelting process through vacuum suspension smelting; the invention uses cooling water to ensure that the copper crucible wall must be cut along the axial direction of the copper crucible, thereby ensuring that the magnetic field generated by the induction coil surrounding the crucible can enter the copper crucible, thereby avoiding the copper crucible from being melted at high temperature; the beryllium titanium alloy of the invention has uniform microstructure composition, high purity, no pore defects, and excellent mechanical properties, thus meeting the performance requirements of the nuclear reactor sheath layer material and improving the compatibility of the nuclear reactor sheath layer material with stainless steel. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Embodiment 1:
[0026] 1) Raw material preparation: Weigh 99.99% pure beryllium flakes and 99.999% pure titanium particles according to the mass percentage of 89wt% and 11wt% respectively. Place the weighed beryllium flakes and titanium particles in a copper crucible, and then fix the copper crucible with a size of 50*120mm in a smelting furnace.
[0027] 2) Vacuuming: Close the suspension furnace door, turn on the power of the control cabinet, turn on the air compressor, turn on the automatic vacuum to extract the air from the furnace, turn on the circulating water of the copper crucible and coil, turn on the water cooler, after 4 minutes, turn on the vacuum gauge, and wait for the vacuum to reach 5×10 - 3 Pa, turn off the vacuum gauge.
[0028] 3) Suspension smelting: open the argon bottle, close the main pumping valve, continue to fill the smelting furnace with argon to below -50Pa, close the charging valve, start the smelting furnace control cabinet, adjust the power knob to 170Kw, and heat up to 1400℃ at a heating rate of 45℃ / min. Vacuum suspension smelting for 20min to obtain suspension smelting liquid.
[0029] 4) Orderly cooling: adjust the power knob, control the cooling rate (30-40℃ / min) 35℃ / min, until the temperature drops to 200℃ (that is, the power is zero), cool for 40 minutes and then form, turn off the power adjustment knob, turn off the power of the control cabinet, turn off the power switch, and then perform surface polishing.
[0030] The Be content of the beryllium-titanium alloy in this embodiment is 89wt%, and the Ti content is 11wt%. According to the test, the longitudinal linear expansion coefficient of the beryllium-titanium alloy in this embodiment is 14.09×10 -6 / ℃, the transverse linear expansion coefficient is 13.16×10 -6 / ℃.
[0031] Embodiment 2:
[0032] 1) Raw material preparation: Weigh 99.99% pure beryllium flakes and 99.999% pure titanium particles according to the mass percentage of 84wt% and 16wt% respectively. Place the weighed beryllium flakes and titanium particles in a copper crucible, and then fix the copper crucible with a size of 50*120mm in a smelting furnace.
[0033] 2) Vacuuming: Close the suspension furnace door, turn on the power of the control cabinet, turn on the air compressor, turn on the automatic vacuum to extract the air from the furnace, turn on the circulating water of the copper crucible and coil, turn on the water cooler, and after 3 minutes, turn on the vacuum gauge and wait for the vacuum to reach 3×10 - 3 Pa, turn off the vacuum gauge.
[0034] 3) Suspension smelting: open the argon bottle, close the main pumping valve, continue to fill the smelting furnace with argon to below -60Pa, close the charging valve, start the smelting furnace control cabinet, adjust the power knob to 150Kw, and heat up to 1000℃ at a heating rate of 30℃ / min. Vacuum suspension smelting for 15min to obtain suspension smelting liquid.
[0035] 4) Orderly cooling: adjust the power knob and control the cooling rate to 30℃ / min until the temperature drops to 100℃ (that is, the power is zero). Cool for 30 minutes and then form. Turn off the power adjustment knob, turn off the power of the control cabinet, turn off the power switch, and then perform surface polishing.
[0036] The Be content of the beryllium titanium alloy in this embodiment is 84wt% and the Ti content is 16wt%. According to the test, the longitudinal linear expansion coefficient of the beryllium titanium alloy in this embodiment is 11.09×10 -6 / ℃, the transverse linear expansion coefficient is 10.39×10 -6 / ℃.
[0037] Embodiment 3:
[0038] 1) Raw material preparation: Weigh 99.99% pure beryllium flakes and 99.999% pure titanium particles according to the mass percentage of 88wt% and 12wt% respectively. Place the weighed beryllium flakes and titanium particles in a copper crucible, and then fix the copper crucible with a size of 50*120mm in a smelting furnace.
[0039] 2) Vacuuming: Close the suspension furnace door, turn on the power of the control cabinet, turn on the air compressor, turn on the automatic vacuum to extract the air from the furnace, turn on the copper crucible and coil circulating water, turn on the water cooler, after 5 minutes, turn on the vacuum gauge, and wait for the vacuum to reach 7×10 - 3 Pa, turn off the vacuum gauge.
[0040] 3) Suspension smelting: open the argon bottle, close the main pumping valve, continue to fill the smelting furnace with argon to below -60Pa, close the charging valve, start the smelting furnace control cabinet, adjust the power knob to 180Kw, and heat up to 1600℃ at a heating rate of 60℃ / min. Vacuum suspension smelting for 30min to obtain suspension smelting liquid.
[0041] 4) Orderly cooling: adjust the power knob and control the cooling rate to 40℃ / min until the temperature drops to 300℃ (that is, the power is zero). Cool for 40 minutes and then form. Turn off the power adjustment knob, turn off the power of the control cabinet, turn off the power switch, and then perform surface polishing.
[0042] The Be content of the beryllium titanium alloy in this embodiment is 88wt%, and the Ti content is 12wt%. According to the test, at -50-150°C, the longitudinal linear expansion coefficient of the beryllium titanium alloy in this embodiment is 13.27×10-6 / °C, and the transverse linear expansion coefficient is 12.06×10 -6 / ℃.
[0043] Embodiment 4:
[0044] 1) Raw material preparation: Weigh 99.99% pure beryllium flakes and 99.999% pure titanium particles according to the mass percentage of 70wt% and 30wt% respectively. Place the weighed beryllium flakes and titanium particles in a copper crucible, and then fix the copper crucible with a size of 50*120mm in a smelting furnace.
[0045] 2) Vacuuming: Close the suspension furnace door, turn on the power of the control cabinet, turn on the air compressor, turn on the automatic vacuum to extract the air from the furnace, turn on the copper crucible and coil circulating water, turn on the water cooler, after 4 minutes, turn on the vacuum gauge, and wait for the vacuum to reach 4×10 - 3 Pa, turn off the vacuum gauge.
[0046] 3) Suspension smelting: open the argon bottle, close the main pumping valve, continue to fill the smelting furnace with argon to below -70Pa, close the charging valve, start the smelting furnace control cabinet, adjust the power knob to 160Kw, and heat up to 1200℃ at a heating rate of 50℃ / min. Vacuum suspension smelting (18min) to obtain suspension smelting liquid.
[0047] 4) Orderly cooling: adjust the power knob and control the cooling rate to 36℃ / min until the temperature drops to 250℃ (that is, the power is zero). Cool for 38 minutes and then form. Turn off the power adjustment knob, turn off the power of the control cabinet, turn off the power switch, and then perform surface polishing.
[0048] The Be content of the beryllium titanium alloy in this embodiment is 70wt% and the Ti content is 30wt%. According to the test, at -50-150°C, the longitudinal linear expansion coefficient of the beryllium titanium alloy in this embodiment is 13.53×10-6 / °C, and the transverse linear expansion coefficient is 12.21×10 -6 / ℃.
[0049] Embodiment 5:
[0050] 1) Raw material preparation: Weigh 99.99% pure beryllium flakes and 99.999% pure titanium particles according to the mass percentage of 82wt% and 18wt% respectively. Place the weighed beryllium flakes and titanium particles in a copper crucible, and then fix the copper crucible with a size of 50*120mm in a smelting furnace.
[0051] 2) Vacuuming: Close the suspension furnace door, turn on the power of the control cabinet, turn on the air compressor, turn on the automatic vacuum to extract the air from the furnace, turn on the circulating water of the copper crucible and coil, turn on the water cooler, after 4 minutes, turn on the vacuum gauge, and wait for the vacuum to reach 6×10 - 3 Pa, turn off the vacuum gauge.
[0052] 3) Suspension smelting: open the argon bottle, close the main pumping valve, continue to fill the smelting furnace with argon to below -65Pa, close the charging valve, start the smelting furnace control cabinet, adjust the power knob to 165Kw, and heat up to 1500℃ at a heating rate of 55℃ / min. Vacuum suspension smelting for 20min to obtain suspension smelting liquid.
[0053] 4) Orderly cooling: adjust the power knob, control the cooling rate (36℃ / min, until the temperature drops to 150℃ (that is, the power is zero), cool for 32 minutes and then form, turn off the power adjustment knob, turn off the power of the control cabinet, turn off the power switch, and then perform surface polishing.
[0054] The Be content of the beryllium titanium alloy in this embodiment is 82wt%, and the Ti content is 18wt%. According to the test, at -50-150°C, the longitudinal linear expansion coefficient of the beryllium titanium alloy in this embodiment is 13.23×10-6 / °C, and the transverse linear expansion coefficient is 12.45×10-6 / °C. -6 / ℃.
[0055] Please note that the technical features of the above embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the technical features in the above embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. The above embodiments only express several implementation methods of the present application, and their descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several variations and improvements can be made, which all belong to the scope of protection of the present application. Therefore, the scope of protection of the patent in this application shall be based on the attached claims.
Claims
1. A method for preparing beryllium-titanium alloy, characterized in that: The preparation method comprises: Step S1, fixing a copper crucible with beryllium sheets and titanium particles in a smelting furnace, water cooling for 3 to 5 minutes and then evacuating, and then continuously filling the smelting furnace with argon until the vacuum pressure in the smelting furnace is -70 to -50 Pa, heating up to 1000 to 1600° C. at a heating rate of 30 to 60° C. / min, and vacuum suspension smelting for 15 to 30 minutes to obtain a suspension smelting liquid; In the step S1, the mass percentages of the beryllium sheets and the titanium particles are 70-89wt% and 11-30wt% respectively; Step S2, cooling the suspension smelting liquid to a temperature of 100 to 300° C. at a cooling rate of 30 to 40° C. / min, cooling the smelted liquid to form the product, and then performing surface polishing.
2. The preparation method according to claim 1, characterized in that: In the step S1, the purity of the beryllium sheet is 99.99%; the purity of the titanium particles is 99.999%.
3. The preparation method according to claim 2, characterized in that: In step S1, the vacuum degree in the evacuated smelting furnace is 3 to 7 × 10 -3 Pa; The vacuum suspension smelting is carried out at a temperature of 1100 to 1500° C. and for a time of 18 to 27 minutes.
4. The preparation method according to claim 3, characterized in that: In step S1, the vacuum degree in the evacuated smelting furnace is 4.4-5.5×10 -3 Pa; The vacuum suspension smelting is carried out at a temperature of 1200 to 1400° C. and for a time of 20 to 24 minutes.
5. The preparation method according to any one of claims 1 to 4, characterized in that: In the step S1, the heating rate is 35-55°C / min.
6. The preparation method according to claim 5, characterized in that: In the step S1, the heating rate is 40-50°C / min.
7. The preparation method according to claim 6, characterized in that: In the step S2, the cooling molding temperature is 150-250°C, and the cooling molding time is 30-50 minutes.
8. A beryllium-titanium alloy, characterized in that: The beryllium-titanium alloy is prepared by the preparation method described in any one of claims 1 to 7.
9. The beryllium-titanium alloy according to claim 8, characterized in that: At -50 to 350°C, the longitudinal linear expansion coefficient of the beryllium-titanium alloy is 11.09×10 -6 / ℃~14.09×10 -6 / ℃, the transverse linear expansion coefficient is 10.39×10 -6 / ℃~13.16×10 -6 / ℃.
Citation Information
Patent Citations
Method for preparing beryllium-titanium alloy by carrying out spark plasma sintering
CN104630524A