Ti-doped Heusler alloy for improving reversible magnetothermal effect of Ni-Co-Mn-Sb-In and preparation method of Ti-doped Heusler alloy

By doping Ti elements in Ni-Co-Mn-Sb-In alloy, the reversible magnetomartensite phase transformation and magnetothermal effect of the alloy are improved, and the magneto-thermal effect of the existing Ni-Mn-Sb-based alloy is solved. The problem of irreversible thermal effect achieves a more efficient magnetic refrigeration effect.

CN118957382APending Publication Date: 2024-11-15NANCHANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410982840.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing Ni-Mn-Sb Kihasler alloy is irreversible during the field cycle of rising magnetic fields and falling magnetic fields, resulting in the disappearance or decrease of magnetothermal effects, limiting its industrial in the field of magnetic refrigeration. application.

Method used

By doping Ti elements in Ni-Co-Mn-Sb-In alloys, the reversibility of magnetomartensite phase transformation and magnetothermal effect was improved, and alloys such as Ni50-x-yTixCoyMn40Sb6In4 or Ni42-xTixCo8Mn40Sb6In4 were prepared, and arc melting was used. and heat treatment method to realize reversible magnetomartensite phase transformation and magnetic entropy transformation of the alloy under a 5 T magnetic field.

Benefits of technology

It significantly improves the reversible magneto-thermal effect of the alloy, increases the reversible magnetic entropy change range under the 5 T magnetic field, and broadens the application range of the alloy, making it an efficient magnetic refrigeration material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957382A_ABST
    Figure CN118957382A_ABST
Patent Text Reader

Abstract

The invention discloses a Ti-doped Heusler alloy for improving the reversible magnetothermal effect of Ni-Co-Mn-Sb-In and a preparation method of the Ti-doped Heusler alloy, and belongs to the technical field of magnetic materials. The chemical formula of the Ni-Ti-Co-Mn-Sb-In Heusler alloy is Ni < 50-x-y > Ti < x > Co < y > Mn < 40 > Sb < 6 > In < 4 >, the sum of atomic percentages in the alloy is 100%, x is larger than or equal to 1.5 and smaller than or equal to 2.5, and y is larger than or equal to 6 and smaller than or equal to 8. The preparation method comprises the following steps: weighing the raw materials according to the proportion, preparing a polycrystalline alloy cast ingot through repeated overturning smelting in a vacuum arc furnace, annealing under the protection of high-purity argon, and then quenching in cold water, thereby preparing the Ni-Ti-Co-Mn-Sb-In Heusler alloy material. According to the alloy disclosed by the invention, under a 5T magnetic field, the volume fraction change range of austenite capable of generating reversible magnetic martensite phase change is 65.7%-92.9%, and the range of reversible magnetic entropy change is 15.9-16.8 J / kg.K. According to the invention, the Ti element is doped, so that the reversibility and reversible magnetic entropy change of magnetic martensite phase transformation in the alloy are improved; compared with the existing Ni-Mn-Sb-based alloy, the Ni-Ti-Co-Mn-Sb-In Heusler alloy disclosed by the invention has higher reversible magnetic martensite phase transformation and a large reversible magnetocaloric effect, and can be used in the field of magnetic refrigeration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of magnetic materials, and in particular relates to a Ti-doped Heusler alloy with improved reversible magnetocaloric effect of Ni-Co-Mn-Sb-In and a preparation method thereof. Background Art

[0002] Traditional gas compression refrigeration technology has been widely used in all walks of life, but it has two obvious defects: first, the refrigeration efficiency is low, and the Carnot cycle efficiency is only 5%~10%; second, the refrigerant used will cause environmental problems such as "ozone hole" and "greenhouse effect". Therefore, finding an efficient, energy-saving and environmentally friendly alternative refrigeration solution is the tireless pursuit of scientists. Unlike traditional gas compression refrigeration technology, magnetic refrigeration uses magnetic solid materials as refrigerants and will not cause environmental problems such as "ozone hole" and "greenhouse effect". In addition, magnetic refrigeration technology has high refrigeration efficiency, and its Carnot cycle efficiency can reach 30%~60%. Based on the above advantages, magnetic refrigeration technology has great potential to replace traditional compression refrigeration technology and become one of the high-tech technologies that are being developed internationally.

[0003] In the development of magnetic refrigeration technology, Ni-Mn-Sb-based Heusler alloys have been widely studied. Researchers have found that there is a strong coupling between the lattice freedom and the spin freedom of Ni-Mn-Sb-based Heusler alloys when the martensitic phase transition occurs, so that the magnetocaloric effect is obtained by magnetocaloric phase transition under the action of a magnetic field. At present, domestic and foreign researchers have carried out a lot of research on the optimization and preparation of the magnetocaloric effect of Ni-Mn-Sb-based alloys, and have developed alloys with large magnetocaloric effect. For Ni-Mn-Sb-based alloys, a large magnetocaloric effect can usually be obtained during the first magnetic field increase process. However, in the subsequent field cycling process of decreasing magnetic field and increasing magnetic field, the magnetocaloric effect disappears or becomes smaller due to the irreversibility or low reversibility of the magnetocaloric phase transition. In fact, magnetocaloric materials need to be used in a cyclic magnetic field of increasing magnetic field and decreasing magnetic field in practical applications. Therefore, only the reversible magnetocaloric effect (the magnetocaloric effect obtained during the second and subsequent field cycles) has practical value. The reversible magnetocaloric effect of the currently reported Ni-Mn-Sb-based alloys under magnetic fields not exceeding 5 T is not ideal, which seriously limits the industrial application of this type of alloy in the field of magnetic refrigeration. Summary of the invention

[0004] In view of the content of the background technology, the purpose of the present invention is to provide a Heusler alloy with improved reversible magnetocaloric effect of Ni-Co-Mn-Sb-In by Ti doping and a preparation method thereof; in the Ni-Co-Mn-Sb-In alloy, the present invention improves the reversibility of magnetocaloric effect and magneto-martensitic phase transformation by replacing Ni element with Ti element, thereby broadening the application scope of the alloy.

[0005] The technical solution of the present invention is as follows: The invention provides a Ti-doped Heusler alloy for improving the reversible magnetocaloric effect of Ni-Co-Mn-Sb-In, wherein the chemical molecular formula of the alloy is Ni 50-x-y Ti x Co y Mn 40 Sb6In4, the sum of the percentages of the elements in the alloy is 100%, where 1.5≤ x ≤ 2.5, 6 ≤ y ≤ 8.

[0006] Furthermore, the chemical formula of the alloy is Ni 42-x Ti x Co8Mn 40 Sb6In4, where 1.5 ≤ x ≤2.5.

[0007] Furthermore, the chemical formula of the alloy is Ni 40.5 Ti 1.5 Co8Mn 40 Sb6In4 or Ni 40 Ti2Co8Mn 40 Sb6In4; Under a 5 T magnetic field, the volume fraction of austenite in the alloy material that can undergo reversible magneto-martensitic transformation varies in the range of 65.7%-92.9%, and the reversible magnetic entropy change varies in the range of 15.9-16.8 J / kg·K.

[0008] The present invention also provides a method for preparing the above-mentioned Ti-doped Ni-Co-Mn-Sb-In Hessler alloy with improved reversible magnetocaloric effect, comprising the following steps: 1) Raw material ratio: The raw materials are prepared according to the atomic percentage of the chemical molecular formula; the purity of Ni, Ti, Mn, Sb and In in the raw materials is 99.99 wt.%, and the purity of Co is 99.98 wt.%; 2) Preparation of alloy ingots: Place the raw materials prepared in step 1) into a water-cooled copper mold in an arc melting furnace, and evacuate the chamber of the arc furnace to a vacuum of 5×10 ‒3 After the temperature reaches 4000 Pa, argon gas of 0.05 MPa is filled in, and arc melting is carried out under electromagnetic stirring. The melting is repeated 5 times to obtain a polycrystalline ingot of Ni-Ti-Co-Mn-Sb-In alloy. 3) Heat treatment: The Ni-Ti-Co-Mn-Sb-In alloy ingot obtained in step 2) is placed in a quartz tube, which is then evacuated and backfilled with argon; the quartz tube containing the alloy ingot is placed in a heat treatment furnace at 1173 K for 9 h, and then quenched in cold water to obtain the Ni-Ti-Co-Mn-Sb-In Heusler alloy.

[0009] Compared with the prior art, the present invention has the following beneficial effects: 1) Doping with Ti element increases Ni 42 Co8Mn 40 Reversibility of magnetocaloric effect and magneto-martensitic transformation in Sb6In4 alloy. 40.5 Ti 1.5 Co8Mn 40 Sb6In4 alloy and Ni 40 Ti2Co8Mn 40 The reversible magnetic entropy changes of Sb6In4 alloy under 5 T magnetic field are 15.9 J / kg·K and 16.8 J / kg·K respectively. Compared with the Ni-Mn-Sb-based alloys reported so far, the alloy of the present invention has higher reversibility of martensitic phase transformation and larger reversible magnetocaloric effect, and is a magnetic refrigeration alloy with great application prospects.

[0010] 2) The raw materials Ni, Ti, Co, Mn, Sb and In required for the Heusler alloy of the present invention are low in price and are ideal candidate materials for non-rare earth magnetic refrigeration. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 For you 42 Co8Mn 40 DSC curve of Sb6In4 alloy.

[0012] Figure 2 For you 40.5 Ti 1.5 Co8Mn 40 DSC curve of Sb6In4 alloy.

[0013] Figure 3 For you 42 Co8Mn 40 Isothermal magnetization curves M(H) of Sb6In4 alloy at different temperatures, where the solid line is the M(H) curve obtained during the first cycle of increasing and decreasing magnetic field, and the dotted line is the M(H) curve obtained during the second cycle of increasing and decreasing magnetic field.

[0014] Figure 4 For you 40.5 Ti 1.5 Co8Mn 40 Isothermal magnetization curves M(H) of Sb6In4 alloy at different temperatures, where the solid line is the M(H) curve obtained during the first cycle of increasing and decreasing magnetic field, and the dotted line is the M(H) curve obtained during the second cycle of increasing and decreasing magnetic field.

[0015] Figure 5 For you 42 Co8Mn 40Magnetic entropy change-temperature curve of Sb6In4 alloy, where the solid symbols represent the maximum magnetic entropy change obtained by the alloy during the first increase in magnetic field to 5 T, and the hollow symbols represent the maximum magnetic entropy change obtained by the alloy during the second increase in magnetic field to 5 T.

[0016] Figure 6 For you 40.5 Ti 1.5 Co8Mn 40 Magnetic entropy change-temperature curve of Sb6In4 alloy, where the solid symbols represent the maximum magnetic entropy change obtained by the alloy during the first increase in magnetic field to 5 T, and the hollow symbols represent the maximum magnetic entropy change obtained by the alloy during the second increase in magnetic field to 5 T.

[0017] Figure 7 For you 40 Ti2Co8Mn 40 DSC curve of Sb6In4 alloy.

[0018] Figure 8 For you 40 Ti2Co8Mn 40 Isothermal magnetization curves M(H) of Sb6In4 alloy at different temperatures, where the solid line is the M(H) curve obtained during the first cycle of increasing and decreasing magnetic field, and the dotted line is the M(H) curve obtained during the second cycle of increasing and decreasing magnetic field.

[0019] Fig. 9 For you 40 Ti2Co8Mn 40 Magnetic entropy change-temperature curve of Sb6In4 alloy, where the solid symbols represent the maximum magnetic entropy change obtained by the alloy during the first increase in magnetic field to 5 T, and the hollow symbols represent the maximum magnetic entropy change obtained by the alloy during the second increase in magnetic field to 5 T. DETAILED DESCRIPTION

[0020] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be clearly and completely described below in conjunction with the embodiments. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.

[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0022] In the following embodiments, Ni is 99.99 wt.% high-purity Ni, Co is 99.98 wt.% high-purity Co, Mn is 99.99 wt.% high-purity Mn, Sb is 99.99 wt.% high-purity Sb, In is 99.99 wt.% high-purity In, and Ti is 99.99 wt.% high-purity Ti.

[0023] The electric arc furnace used was purchased from Shenyang Haozhiduo New Materials Preparation Technology Co., Ltd., and the model of the electric arc furnace is HVAM-B.

[0024] The detection technology means adopted in the embodiment are: A cylinder with a size of Φ3mm×0.3mm was cut from the prepared alloy button ingot by wire cutting, and then its surface was polished clean with sandpaper as a test sample. The martensitic phase transition temperature, reverse martensitic phase transition temperature and phase transition entropy change Δ of the reverse martensitic phase transition were measured by differential scanning calorimetry (DSC). S A The heating rate and cooling rate during the DSC test were both 10 K / min. The phase entropy change (Δ S A ) can be calculated by the following formula:

[0025] Among them, T1 and T2 are the phase transition start temperature and phase transition end temperature respectively.

[0026] The isothermal magnetization curve of the sample was measured by a comprehensive physical property measurement system (PPMS). The isothermal magnetization curve at each temperature was measured as follows: (1) the temperature was lowered to below the martensitic phase transition temperature, and then the temperature was raised to the target temperature; (2) the magnetic field was then raised to 5 T, lowered to 0 T, raised to 5 T, and lowered to 0 T to obtain the M(H) curve of the alloy sample. The reversible magnetocaloric effect of the alloy can be obtained by the magnetic entropy change-temperature curve (Δ S m - T curve) to characterize the sample’s Δ S m (Magnetic entropy change) can be calculated by the following formula:

[0027] Among them, M(H i ) is the sample in a magnetic field of H i The magnetization intensity at M (H i ) is pure martensite in a magnetic field of H i The magnetization intensity at A (H i) is pure austenite in a magnetic field of H i The magnetization intensity, M(H f ) is the sample in a magnetic field of H f The magnetization intensity at M (H f ) is pure martensite in a magnetic field of H f The magnetization intensity at A (H f ) is pure austenite in a magnetic field of H f The magnetization intensity at .

[0028] Example 1Ni 40.5 Ti 1.5 Co8Mn 40 Sb6In4 alloy 1. Ingredients: According to Ni 42 Co8Mn 40 Sb6In4 and Ni 40.5 Ti 1.5 Co8Mn 40 The atomic percentage of Sb6In4 is as follows: High-purity Ni, Co, Mn, Sb, In and Ti metal elements are weighed, and the purity of Ni, Mn, Sb, In and Ti is 99.99 wt.%, and the purity of Co is 99.98 wt.%.

[0029] 2. Preparation of alloy button ingots: Put the Ni, Co, Mn, Sb, In and Ti metal elements weighed in step 1 into a vacuum arc melting furnace, and evacuate the arc furnace chamber to 5×10 -3 Pa, and then filled with high-purity argon gas 0.05 MPa; electromagnetic stirring was used to stir the alloy liquid during the arc melting process, and after the alloy liquid solidified, the alloy ingot was turned over by a mechanical gripper; the above arc melting process was repeated 5 times to obtain Ni 42 Co8Mn 40 Sb6In4 alloy and Ni 40.5 Ti 1.5 Co8Mn 40 Button ingot of Sb6In4 alloy.

[0030] 3. Heat treatment: Ni 42 Co8Mn 40 Sb6In4 alloy and Ni 40.5 Ti 1.5 Co8Mn 40 The button ingot of Sb6In4 alloy was placed in a quartz tube, which was then evacuated and backfilled with high-purity argon gas. The quartz tube containing the alloy button ingot was placed in a heat treatment furnace at 1173 K for 9 h, and then quenched in cold water to obtain Ni 42 Co8Mn 40 Sb6In4 alloy and Ni40.5 Ti 1.5 Co8Mn 40 Sb6In4 alloy.

[0031] 4. Use DSC to measure the martensitic transformation temperature, reverse martensitic transformation temperature and the phase entropy change of the martensitic transformation of the alloy sample. 42 Co8Mn 40 The DSC curve of Sb6In4 alloy is as follows Figure 1 As shown, Ti-doped Ni 40.5 Ti 1.5 Co8Mn 40 The DSC curve of Sb6In4 alloy is as follows Figure 2 As the temperature increases from 372 K to 396 K, the Ni 42 Co8Mn 40 The Sb6In4 alloy transforms from martensite to austenite; when the temperature is cooled from 386 K to 359 K, the Ni 42 Co8Mn 40 Sb6In4 alloy transforms from austenite to martensite; Ni 42 Co8Mn 40 The phase transition entropy of the reverse martensitic transformation in Sb6In4 alloy is 40.4 J / kg·K. As the temperature increases from 270 K to 308 K, the Ni doped with Ti 40.5 Ti 1.5 Co8Mn 40 The Sb6In4 alloy transforms from martensite to austenite; during the temperature drop from 295 K to 266 K, the Ti-doped Ni 40.5 Ti 1.5 Co8Mn 40 Sb6In4 alloy transforms from austenite to martensite; Ti-doped Ni 40.5 Ti 1.5 Co8Mn 40 The phase transformation entropy of the reverse martensitic transformation in Sb6In4 alloy is 24.2 J / kg·K.

[0032] 5. Use PPMS to measure the isothermal magnetization curves M(H) of the alloy samples at different temperatures. 42 Co8Mn 40 The isothermal magnetization curve M(H) of Sb6In4 alloy obtained during two consecutive cycles of increasing and decreasing magnetic fields is shown in Figure 3 As shown. Ti-doped Ni 40.5 Ti 1.5 Co8Mn 40The isothermal magnetization curve M(H) of Sb6In4 alloy obtained during two consecutive cycles of increasing and decreasing magnetic fields is shown in Figure 4 In the range of 380 K to 386 K, Ni 42 Co8Mn 40 The magneto-induced martensitic transformation of Sb6In4 alloy under 5 T magnetic field is partially reversible, but the reversibility of magneto-induced martensitic transformation is low. 40.5 Ti 1.5 Co8Mn 40 The magneto-induced martensitic transformation of Sb6In4 alloy under 5 T magnetic field also shows partially reversible characteristics, but the reversibility of magneto-induced martensitic transformation is higher.

[0033] 6. Figure 5 It's Ni 42 Co8Mn 40 Magnetic entropy change-temperature curve of Sb6In4 alloy obtained during two consecutive cycles of increasing and decreasing magnetic field. 42 Co8Mn 40 The maximum magnetic entropy change of Sb6In4 alloy in the first field cycle is 34.9 J / kg·K, and the maximum magnetic entropy change in the second field cycle is reduced to 7 J / kg·K, that is, the maximum reversible magnetic entropy change is 7 J / kg·K. 42 Co8Mn 40 The maximum volume fraction of austenite that can undergo reversible magneto-martensitic transformation in the Sb6In4 alloy sample is 17.3%. Figure 6 It's Ni 40.5 Ti 1.5 Co8Mn 40 Magnetic entropy change-temperature curve of Sb6In4 alloy obtained during two consecutive cycles of increasing and decreasing magnetic field. 40.5 Ti 1.5 Co8Mn 40 The maximum magnetic entropy change of Sb6In4 alloy during the first field cycle was 21.6 J / kg·K, and the maximum magnetic entropy change during the second field cycle dropped to 15.9 J / kg·K, that is, the maximum reversible magnetic entropy change was 15.9 J / kg·K. 40.5 Ti 1.5 Co8Mn 40 The maximum volume fraction of austenite that can undergo reversible magneto-martensitic transformation in the Sb6In4 alloy sample is 65.7%. The above results show that Ti doping improves the reversibility of magneto-martensitic transformation in the alloy and increases the reversible magnetic entropy change of the alloy.

[0034] Example 2Ni40 Ti2Co8Mn 40 Sb6In4 alloy 1. Ingredients: According to Ni 42 Co8Mn 40 Sb6In4 and Ni 40 Ti2Co8Mn 40 The atomic percentage of Sb6In4 is as follows: High-purity Ni, Co, Mn, Sb, In and Ti metal elements are weighed, and the purity of Ni, Mn, Sb, In and Ti is 99.99 wt.%, and the purity of Co is 99.98 wt.%.

[0035] 2. Preparation of alloy button ingots: Put the Ni, Co, Mn, Sb, In and Ti metal elements weighed in step 1 into a vacuum arc melting furnace, and evacuate the arc furnace chamber to 5×10 -3 Pa, and then high-purity argon gas was filled to 0.05 MPa; electromagnetic stirring was used to stir the alloy liquid during the arc melting process, and after the alloy liquid solidified, a mechanical gripper was used to flip the alloy ingot; the above arc melting process was repeated 5 times to obtain Ni 42 Co8Mn 40 Sb6In4 alloy and Ni 40 Ti2Co8Mn 40 Button ingot of Sb6In4 alloy.

[0036] 3. Heat treatment: Ni 42 Co8Mn 40 Sb6In4 alloy and Ni 40 Ti2Co8Mn 40 The button ingot of Sb6In4 alloy was placed in a quartz tube, which was then evacuated and backfilled with high-purity argon gas. The quartz tube containing the alloy button ingot was placed in a heat treatment furnace at 1173 K for 9 h, and then quenched in cold water to obtain Ni 42 Co8Mn 40 Sb6In4 alloy and Ni 40 Ti2Co8Mn 40 Sb6In4 alloy.

[0037] 4. Use DSC to measure the martensitic transformation temperature, reverse martensitic transformation temperature and the phase entropy change of the martensitic transformation of the alloy sample. 42 Co8Mn 40 The DSC curve of Sb6In alloy is as follows Figure 1 As shown, Ti-doped Ni 40 Ti2Co8Mn 40 The DSC curve of Sb6In4 alloy is as follows Figure 7As the temperature increases from 372 K to 396 K, the Ni 42 Co8Mn 40 The Sb6In4 alloy transforms from martensite to austenite; when the temperature is cooled from 386 K to 359 K, the Ni 42 Co8Mn 40 Sb6In4 alloy transforms from austenite to martensite; Ni 42 Co8Mn 40 The phase transition entropy of the reverse martensitic transformation in the Sb6In4 alloy is 40.4 J / kg·K. As the temperature increases from 202 K to 222 K, the Ni doped with Ti 40 Ti2Co8Mn 40 The Sb6In4 alloy transforms from martensite to austenite; during the cooling process from 205 K to 175 K, the Ti-doped Ni 40 Ti2Co8Mn 40 Sb6In4 alloy transforms from austenite to martensite; Ti-doped Ni 40 Ti2Co8Mn 40 The phase transformation entropy of the reverse martensitic transformation in Sb6In4 alloy is 18.0 J / kg·K.

[0038] 5. Use PPMS to measure the isothermal magnetization curves M(H) of the samples at different temperatures. 42 Co8Mn 40 The isothermal magnetization curve M(H) of Sb6In4 alloy obtained during two consecutive cycles of increasing and decreasing magnetic fields is shown in Figure 3 As shown. Ti-doped Ni 40 Ti2Co8Mn 40 The isothermal magnetization curve M(H) of Sb6In4 alloy obtained during two consecutive cycles of increasing and decreasing magnetic fields is shown in Figure 8 In the range of 380 K to 386 K, Ni 42 Co8Mn 40 The magneto-induced martensitic transformation of Sb6In4 alloy under 5 T magnetic field is partially reversible, but the reversibility of magneto-induced martensitic transformation is low. 40 Ti2Co8Mn 40 The magneto-induced martensitic transformation of Sb6In4 alloy under 5 T magnetic field also shows partially reversible characteristics, and the reversibility of magneto-induced martensitic transformation is relatively high.

[0039] 6. Figure 5 It's Ni 42 Co8Mn40 Magnetic entropy change-temperature curve of Sb6In4 alloy obtained during two consecutive cycles of increasing and decreasing magnetic field. 42 Co8Mn 40 The maximum magnetic entropy change of Sb6In4 alloy in the first field cycle is 34.9 J / kg·K, and the maximum magnetic entropy change in the second field cycle is reduced to 7 J / kg·K, that is, the maximum reversible magnetic entropy change is 7 J / kg·K. 42 Co8Mn 40 The maximum volume fraction of austenite that can undergo reversible magneto-martensitic transformation in the Sb6In4 alloy sample is 17.3%. Fig. 9 It's Ni 40 Ti2Co8Mn 40 Magnetic entropy change-temperature curve of Sb6In4 alloy obtained during two consecutive cycles of increasing and decreasing magnetic field. 40 Ti2Co8Mn 40 The maximum magnetic entropy change of Sb6In4 alloy in the first field cycle is 17.8 J / kg·K, and the maximum magnetic entropy change in the second field cycle is reduced to 16.8 J / kg·K, that is, the maximum reversible magnetic entropy change is 16.8 J / kg·K. 40 Ti2Co8Mn 40 The maximum volume fraction of austenite that can undergo reversible magneto-martensitic transformation in the Sb6In4 alloy sample is 93.3%. The above results show that Ti doping improves the reversibility of magneto-martensitic transformation in the alloy and increases the reversible magnetic entropy change of the alloy.

[0040] The embodiments described above only express several preferred embodiments of the present invention, and the descriptions thereof are relatively specific and detailed, but are not intended to limit the present invention. It should be noted that for those skilled in the art, the present invention may also have various changes and modifications, and any modifications, equivalent substitutions, improvements, etc. made within the concept and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A Ti-doped Ni-Co-Mn-Sb-In Heusler alloy with improved reversible magnetocaloric effect, characterized in that: The chemical formula of the alloy is Ni 50-x-y Ti x Co y Mn 40 Sb6In4, the sum of the percentages of the elements in the alloy is 100%, where 1.5 ≤x ≤ 2.5, 6 ≤ y ≤ 8.

2. The Ti-doped Heusler alloy for improving the reversible magnetocaloric effect of Ni-Co-Mn-Sb-In according to claim 1, characterized in that: The chemical formula of the alloy is Ni 42-x Ti x Co8Mn 40 Sb6In4, where 1.5 ≤ x ≤ 2.

5.

3. The Ti-doped Heusler alloy for improving the reversible magnetocaloric effect of Ni-Co-Mn-Sb-In according to claim 1, characterized in that: The chemical formula of the alloy is Ni 40.5 Ti 1.5 Co8Mn 40 Sb6In4 or Ni 40 Ti2Co8Mn 40 Sb6In4; Under a 5T magnetic field, the volume fraction of austenite in the alloy material that can undergo reversible magneto-martensitic transformation varies in the range of 65.7%-92.9%, and the reversible magnetic entropy change varies in the range of 15.9-16.8 J / kg·K.

4. The method for preparing the Ti-doped Heusler alloy for improving the reversible magnetocaloric effect of Ni-Co-Mn-Sb-In according to any one of claims 1 to 3, characterized in that: The steps include: 1) Raw material ratio: The raw materials are prepared according to the atomic percentage of the chemical molecular formula; the purity of Ni, Ti, Mn, Sb and In in the raw materials is 99.99 wt.%, and the purity of Co is 99.98 wt.%; 2) Preparation of alloy ingots: Place the raw materials prepared in step 1) into a water-cooled copper mold in an arc melting furnace, and evacuate the chamber of the arc furnace to a vacuum of 5×10 ‒3 After the temperature reaches 4000 Pa, argon gas of 0.05 MPa is filled in, and arc melting is carried out under electromagnetic stirring. The melting is repeated 5 times to obtain a polycrystalline ingot of Ni-Ti-Co-Mn-Sb-In alloy. 3) Heat treatment: The Ni-Ti-Co-Mn-Sb-In alloy ingot obtained in step 2) is placed in a quartz tube, which is then evacuated and backfilled with argon; the quartz tube containing the alloy ingot is placed in a heat treatment furnace at 1173 K for 9 h, and then quenched in cold water to obtain the Ni-Ti-Co-Mn-Sb-In Heusler alloy.