Corrosion-resistant high-strength and high-toughness steel with tensile strength of 460 MPa and production method of corrosion-resistant high-strength and high-toughness steel
By adjusting chemical composition and production process, high-strength and high-tough steel with tensile strength of 460MPa grade was prepared, which solved the problem that the existing technology could not meet the corrosion resistance and strength requirements of the spokes of mine trucks, and achieved high strength, toughness and corrosion resistance. Matching, reducing corrosion rate, suitable for mine truck spokes.
Patent Information
- Application Number
- CN202411218391.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art cannot provide high-strength and high-toughness steel with tensile strength of 460MPa grade, and has good corrosion resistance, which is suitable for the needs of spokes of mine trucks.
By adjusting the chemical composition and production process, the chemical composition of the steel is C0.05-0.16%, Si≤0.50%, Mn 1.0-1.5%, P≤0.030%, S≤0.010%, Nb 0.025-0.060%, Ti0. 030~0.050%, Sb 0.02~0.30%, Al 0.45~1.0%, the balance is balanced iron and inevitable impurities. Heating, rough rolling, finishing rolling and high-cooling fast cooling technology are used to control grain size and structure .
The yield strength of steel is ≥340MPa, tensile strength of 460~600MPa, elongation rate of ≥30%, impact work of -20℃ ≥200J, corrosion rate relative to Q355B is ≤5%, and has excellent corrosion resistance and is suitable for ore spokes.
Smart Images

Figure BDA0005022226830000041 
Figure BDA0005022226830000051
Abstract
Description
Technical Field
[0001] The invention relates to a high-strength and high-toughness steel with a tensile strength of 460 MPa and corrosion resistance and a production method thereof, belonging to the technical field of low-alloy high-strength steel production. Background Art
[0002] With the development of the infrastructure industry and the demand for large-scale engineering construction, the application of mining trucks is increasing. Mining trucks and other vehicles are used in harsh conditions, and the service reliability of various vehicle components is required to be high. The wheel is the moving component of the vehicle and carries a large load. In particular, mining trucks are used in harsh conditions. In order to ensure the service reliability of mining truck spokes, the material is required to have good strength and toughness, and at the same time have the performance of acid-washing soil corrosion resistance.
[0003] The document with Chinese patent application number: CN202011378962.2 discloses a 540MPa grade thick gauge automobile wheel spoke steel, which includes: 0.05-0.10wt% C, 1.00-2.00wt% Mn, 0.05-0.30wt% Si, 0.02-0.05wt% Nb, 0.01-0.05wt% Ti, 0.01-0.05wt% Als, P≤0.020wt%, S≤0.010wt%, and the balance is Fe; its metallographic structure is ferrite + pearlite, yield strength ≥450MPa, tensile strength ≥540MPa, elongation ≥20%, 180° cold bending test d=a qualified, and grain size ≥10. The components involved in the preparation of the materials in this patent document do not require corrosion resistance and are not suitable for mining truck wheels.
[0004] The document with Chinese patent application number: CN201410116557.1 discloses steel for heavy truck ultra-thick steel spokes and its production method, with the mass percentage of trace elements: carbon 0.07-0.12%; silicon 0.05-0.15%; manganese 0.7-1.1%; niobium 0.01-0.03%; titanium 0.01-0.03%; phosphorus ≤0.015%; sulfur ≤0.005%; aluminum 0.02-0.05%; nitrogen ≤0.006%. The production method is to obtain a casting billet through KR desulfurization and LF treatment, perform rough rolling and finish rolling, laminar cooling, and coil to obtain the required steel, which meets the requirements of heavy truck wheel spoke steel for easy spinning, surface quality and performance stability, and greatly reduces the breakage rate of heavy truck wheels. The materials prepared in this patent document are mainly used for heavy truck wheels, and do not require toughness and corrosion resistance, so they are not suitable for mining truck wheels.
[0005] The document with Chinese patent application number: CN201410786247.0 discloses a 600MPa grade thick gauge hot-rolled spoke steel and its production method, wherein the chemical composition mass percentage of the spoke steel is: 0.06-0.12% C, 0.20-0.60% Si, 0.80-1.20% Mn, 0.02-0.06% Alt, 0.50-1.00% Cr, 0.03-0.08% P, S≤0.005%, N≤0.006%, and the balance is Fe and unavoidable impurities; the billet heating temperature is 1150-1250°C, the finishing rolling temperature is 760-840°C, and the conventional cooling process is adopted after rolling, and the coiling is carried out at a cooling rate of 20-100°C / s to below 350°C. The components involved in the preparation of the materials in this patent document do not have requirements for toughness and corrosion resistance, and are not suitable for mining truck wheels. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a high-strength and high-toughness steel with a tensile strength of 460MPa and corrosion resistance and a production method thereof in view of the deficiencies of the above-mentioned prior art. The steel has a yield strength of ≥340MPa, a tensile strength of 460-600MPa, an elongation of ≥30%, an impact energy of ≥200J at -20℃, a corrosion rate of ≤5% relative to that of Q355B, good corrosion resistance, and is suitable for use in mining truck spokes.
[0007] The technical solution adopted by the present invention to solve the above-mentioned problems is:
[0008] A high-strength and high-toughness steel with a tensile strength of 460MPa and corrosion resistance, the chemical composition of which is as follows by weight percentage: C 0.05-0.16%, Si≤0.50%, Mn 1.0-1.5%, P≤0.030%, S≤0.010%, Nb 0.025-0.060%, Ti0.030-0.050%, Sb 0.02-0.30%, Al 0.45-1.0%, and the balance is balanced iron and inevitable impurities.
[0009] Preferably, the weight percentage of Si is 0.1-0.4%.
[0010] Preferably, the weight percentage of Nb is between 0.035% and 0.055%.
[0011] Preferably, the weight percentage of Sb is 0.05-0.25%.
[0012] Preferably, the weight percentage of Al is between 0.50% and 0.80%.
[0013] The production method of the corrosion-resistant high-strength and high-toughness steel with a tensile strength of 460 MPa of the present invention comprises the following steps:
[0014] 1) Heating the slab: the slab temperature entering the furnace is ≥900°C, and the heating temperature is controlled at 1200-1250°C;
[0015] 2) Rough rolling the heated ingot: the rough rolling end temperature is controlled at 1020-1100°C;
[0016] 3) Finish rolling the slab after rough rolling: control the final rolling temperature at 800-850°C; open the number of cooling water between the stands ≥5;
[0017] 4) After rolling, the steel plate is directly cooled to 480-540°C by water flow at a cooling rate of 60-120°C / s and then coiled to obtain a corrosion-resistant high-strength and high-toughness steel with a tensile strength of 460MPa.
[0018] Preferably, the heating temperature of the casting is controlled at 1200-1230°C.
[0019] Preferably, the cooling rate of the steel plate is 70 to 110° C. / s, and the steel plate is coiled after being cooled to 500 to 540° C.
[0020] The role and reasons for control of the main components and processes in the present invention:
[0021] Carbon: Carbon plays a major role in solid solution strengthening. According to the performance requirements of the steel grade of the present invention, taking both strength and elongation into consideration, the carbon content is limited to 0.05-0.16%.
[0022] Silicon: It mainly plays a deoxidizing role and also has a certain solid solution strengthening effect. However, too high a silicon content will cause the iron oxide scale to adhere to the body, which is not conducive to the removal of the surface iron oxide scale. Therefore, the present invention limits the silicon content to ≤ 0.50%.
[0023] Antimony: Sb can form a Sb2O5 corrosion-resistant oxide film on the steel surface, form SbOCl precipitation and adhesion in the anode micro-area, fill corrosion cracks or voids, improve the ability to block the penetration of corrosive Cl-, and improve the corrosion resistance of steel in environments such as pickling soil; but Sb is easily enriched in the grain boundaries, affecting the formability and toughness of the steel; therefore, the Sb content of the present invention is controlled to be 0.02% to 0.30%, preferably 0.05% to 0.25%.
[0024] Aluminum: The addition of Al can reduce the corrosion current density of steel. The corrosion product forms FeAl2O4 with cation selectivity, which inhibits the formation of Cl -The Al content is controlled to be 0.45% to 1.0%, preferably 0.5% to 0.8%.
[0025] Manganese: Manganese can improve strength and toughness. If its content is less than 1.00%, it cannot meet the material strength requirements; if its content is higher than 1.50%, it will increase the alloy cost of steel. Therefore, the present invention limits the manganese content to 1.00-1.50%.
[0026] Titanium: Under appropriate processes, titanium can exert precipitation strengthening effects, allowing the steel to obtain the desired strength. According to the performance requirements of the steel plate of the present invention, if the titanium content is less than 0.03%, the amount of precipitates is insufficient to support the strength to reach the design lower limit, and if the titanium content is higher than 0.05%, the tensile strength will exceed the upper limit requirement. Therefore, the present invention limits the titanium content to a range of 0.03 to 0.05%.
[0027] Niobium: Niobium is mainly precipitated in steel in the form of Nb (C, N), which prevents the growth of austenite grains, eventually reduces the size of ferrite grains, refines the structure, and thus improves the strength and toughness of steel. When its content is less than 0.025%, the material strength requirement cannot be met; and when the added niobium is higher than 0.060%, the strength requirement can be met. Therefore, the present invention limits the niobium content to the range of 0.025-0.060%.
[0028] Phosphorus and sulfur are harmful elements in steel and their contents must be controlled as required.
[0029] In the present invention, the rolling process of the steel material is to obtain a fine grain size, and further refine the grain size through high cooling rate after rolling, so as to obtain good impact toughness while the material reaches the designed strength.
[0030] Furthermore, the reason why the rough rolling end temperature is controlled at 1020-1100° C. in the present invention is to ensure that the grain size after the rough rolling is not too large.
[0031] The reason why the final rolling temperature of the finishing rolling is controlled at 800-850° C. is to control the grain size of the steel material after the finishing rolling and promote the ferrite phase transformation in the subsequent cooling process.
[0032] The reason why the present invention controls the cooling rate to 60-120°C / s and cools to 480-540°C is that the high cooling rate suppresses the grain growth of the steel plate during the cooling process, and at the same time cools to the target temperature for coiling, ensuring that the steel plate obtains the final required ferrite ratio and grain size.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] The corrosion-resistant high-strength and high-toughness steel with a tensile strength of 460MPa provided by the present invention has good strength and toughness matching, and excellent corrosion resistance. As a steel for the spokes of mining trucks, it can greatly reduce the corrosion rate and increase the service life. Specifically, the steel has a yield strength of ≥340MPa, a tensile strength of 460-600MPa, an elongation of ≥30%, an impact energy of ≥200J at -20℃, and a corrosion rate of ≤5% relative to Q355B steel. DETAILED DESCRIPTION
[0035] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the present invention is not limited to the following embodiments.
[0036] Example
[0037] The following describes each embodiment in detail:
[0038] Table 1 is a list of component values of various embodiments and comparative examples of the present invention;
[0039] Table 2 is a table of process parameter values and performance tests of various embodiments and comparative examples of the present invention;
[0040] Table 3 shows the corrosion resistance test results of various embodiments and comparative examples of the present invention.
[0041] Each embodiment of the present invention is produced according to the following steps:
[0042] 1) Heating the slab: the slab temperature entering the furnace is ≥900°C, and the heating temperature is controlled at 1200-1250°C;
[0043] 2) Rough rolling the heated ingot: the rough rolling end temperature is controlled at 1020-1100°C;
[0044] 3) Finish rolling the slab after rough rolling: control the final rolling temperature at 800-850°C; open the number of cooling water between the stands ≥5;
[0045] 4) After rolling, the steel plate is directly cooled to 480-540°C by water flow at a cooling rate of 60-120°C / s for coiling.
[0046] The production process of the comparative example is carried out with reference to the example, and the specific component values, process parameter values and performance tests are also shown in Tables 1, 2 and 3.
[0047] Table 1 List of chemical components of various embodiments and comparative examples of the present invention (unit: wt%)
[0048] Example C Mn Si Sb Al Ti Nb P S 1 0.121 1.23 0.1 0.02 0.55 0.034 0.033 0.008 0.004 2 0.067 1.10 0.2 0.23 0.80 0.042 0.058 0.011 0.003 3 0.083 1.45 0.1 0.18 0.65 0.05 0.035 0.015 0.003 4 0.05 1.50 0.3 0.25 0.72 0.03 0.045 0.009 0.005 5 0.153 1.31 0.4 0.15 0.62 0.045 0.055 0.015 0.001 6 0.16 1.15 0.3 0.08 0.50 0.037 0.042 0.016 0.002 Comparative Example 0.07 1.62 0.12 0 0.04 0.03 0.031 0.011 0.004
[0049] Table 2 Main process parameters and performance test list of various embodiments and comparative examples of the present invention
[0050]
[0051]
[0052] Table 3 Corrosion resistance test results of various embodiments of the present invention and comparative examples
[0053] category <![CDATA[Total immersion corrosion rate (g / m 2 ·h)]]> Relative corrosion rate (%) Q355B 10.218 100 Example 1 0.452 4.42 Example 2 0.375 3.67 Example 3 0.438 4.29 Example 4 0.396 3.88 Example 5 0.409 4.00 Example 6 0.441 4.32 Comparative Example 2.832 27.72
[0054] Note: Examples 1-6 in Table 2 and Table 3 correspond to Examples 1-6 in Table 1.
[0055] In Table 3, the corrosion performance test was conducted according to the "JB / T7901-1999 Metal Materials Laboratory Uniform Corrosion Full Immersion Test Method", with a temperature of 23±2°C, 10% H2SO4+3.5% NaCl solution, and full immersion for 24 hours, simulating the corrosion of steel by the acidic high-salinity soil leaching solution in the mine. The test results show that the corrosion rate of the steel of the present invention relative to Q355B is within 5%.
[0056] From the results in Table 2 and Table 3 above, it can be seen that the thickness of the steel produced by the present invention is 16-24 mm, the yield strength of the steel is 410-465 MPa, the tensile strength is 530-560 MPa, the elongation is ≥30%, the impact energy at -20°C is ≥210 J, and the corrosion rate relative to Q355B steel is ≤5%. Therefore, the steel produced by the present invention has good corrosion resistance while meeting the requirements of high strength and high toughness, and can be used as steel for mining truck wheel spokes.
[0057] The above is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and changes without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A corrosion-resistant high-strength and high-toughness steel with a tensile strength of 460 MPa, characterized in that: The chemical composition by weight percentage is: C 0.05-0.16%, Si≤0.50%, Mn 1.0-1.50%, P≤0.030%, S≤0.010%, Nb0.025-0.060%, Ti 0.030-0.050%, Sb 0.02-0.30%, Al 0.45-1.0%, and the balance is iron and inevitable impurities.
2. The corrosion-resistant high-strength and high-toughness steel with a tensile strength of 460 MPa according to claim 1, characterized in that: The weight percentage of Si is 0.1-0.4%.
3. The corrosion-resistant high-strength and high-toughness steel with a tensile strength of 460 MPa according to claim 1, characterized in that: The weight percentage of Nb is 0.035-0.055%.
4. The corrosion-resistant high-strength and high-toughness steel with a tensile strength of 460 MPa according to claim 1, characterized in that: The weight percentage of Sb is 0.05-0.25%.
5. The corrosion-resistant high-strength and high-toughness steel with a tensile strength of 460 MPa according to claim 1, characterized in that: The weight percentage of Al is 0.50-0.80%.
6. The method for producing the corrosion-resistant high-strength and high-toughness steel with a tensile strength of 460 MPa as claimed in any one of claims 1 to 5, characterized in that: The following steps are involved: 1) Heating the slab: the slab temperature entering the furnace is ≥900°C, and the heating temperature is controlled at 1200-1250°C; 2) Rough rolling the heated ingot: the rough rolling end temperature is controlled at 1020-1100°C; 3) Finish rolling the slab after rough rolling: control the final rolling temperature at 800-850°C; 4) After rolling, the steel plate is directly cooled to 480-540°C by water flow at a cooling rate of 60-120°C / s and then coiled to obtain a corrosion-resistant high-strength and high-toughness steel with a tensile strength of 460MPa.
7. The method for producing high-strength and high-toughness steel with a tensile strength of 460 MPa and corrosion resistance according to claim 6, characterized in that: The heating temperature of the casting is controlled at 1200-1230℃.
8. The method for producing high-strength and high-toughness steel with a tensile strength of 460 MPa and corrosion resistance according to claim 6, characterized in that: The steel plate is cooled at a rate of 70 to 110°C / s and is coiled after being cooled to 500 to 540°C.
9. The method according to claim 6 produces a corrosion-resistant high-strength and high-toughness steel with a tensile strength of 460 MPa, characterized in that: The thickness of the steel is 16 to 24 mm, the yield strength is ≥340 MPa, the tensile strength is 460 to 600 MPa, the elongation is ≥30%, the impact energy at -20°C is ≥200 J, and the corrosion rate relative to Q355B steel is ≤5%.
10. Use of the high-strength and high-toughness steel according to claim 9 as steel for mining truck wheel spokes.
Citation Information
Patent Citations
540 LF steel strip for 540 Mpa grade automobile spokes and production method of steel strip
CN110484815A
High-performance and hot-rolled wear-resistant steel sheet and production method thereof
CN111254351A
Ultrahigh-strength steel for sanitation trucks and production method thereof
CN111575589A
KR20240098760A