Noise-reduction corrosion-resistant aluminum alloy product as well as preparation process and application thereof
Through the granulation and extrusion wire weaving process of aluminum alloy carbon fiber composite materials, noise reduction and corrosion-resistant aluminum alloy products are formed, which solves the problem of failure and excessive density of porous sound-absorbing materials at high temperatures, and achieves lightweight and efficient sound absorption Combination of performance.
Patent Information
- Application Number
- CN202411038511.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, porous sound-absorbing materials fail at high temperatures or are too dense to meet the needs of lightweighting, which limits their application fields.
Using aluminum alloy carbon fiber composite material, the aluminum alloy powder, carbon fiber and binder are granulated and prepared into extruded wires and weaved into a mesh structure to form noise-reducing and corrosion-resistant aluminum alloy products with a density of 0.05g/ cm3~0.8g/cm3, porosity is 75%~90%, to improve sound absorption performance and corrosion resistance.
It realizes lightweight materials that maintain good sound absorption performance at high temperatures, extends service life, reduces material weight and cost of use, and improves the mechanical properties and corrosion resistance of composite materials.
Smart Images

Figure BDA0004971759960000101 
Figure BDA0004971759960000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloy materials, and in particular to a noise-reducing and corrosion-resistant aluminum alloy product and a preparation process and application thereof. Background Art
[0002] Due to the uniqueness of its internal structure, porous sound-absorbing materials can effectively absorb sound wave energy, thus playing a role in sound insulation and noise reduction. When sound waves enter porous sound-absorbing materials, due to the presence of a large number of tiny gaps and continuous bubbles inside the material, the sound waves encounter the internal friction of the material itself and the friction between the air in the pores and the pore walls inside the material. These frictions will cause the sound wave energy to significantly attenuate during the propagation process. At the same time, because the pores inside the material are continuous, the sound waves will propagate repeatedly in these pores, further increasing the energy loss.
[0003] Polyurethane foam materials are lightweight, environmentally friendly, flame retardant, and easy to cut, making them a commonly used sound insulation and noise reduction material in industry. However, most polyurethane foam materials fail at temperatures above 100°C, limiting their use scenarios. Although most metal porous sound-absorbing materials can be used at high temperatures, due to their high density, their weight per unit volume is dozens of times that of polyurethane foam materials, which cannot meet the demand for lightweighting, limiting the application areas of metal porous sound-absorbing materials.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] One of the purposes of the present invention is to provide a noise-reducing and corrosion-resistant aluminum alloy product to alleviate at least one of the above-mentioned technical problems in the prior art.
[0006] A second object of the present invention is to provide a process for preparing a noise-reducing and corrosion-resistant aluminum alloy product.
[0007] A third object of the present invention is to provide an application of a noise-reducing and corrosion-resistant aluminum alloy product.
[0008] In order to solve the above-mentioned technical problems, the present invention particularly adopts the following technical solutions:
[0009] A first aspect of the present invention provides a noise-reducing and corrosion-resistant aluminum alloy product, which is obtained by weaving fiber filaments of a composite material into a mesh, and then pressing the mesh structure into a desired shape and size;
[0010] Wherein, the composite material is an aluminum alloy carbon fiber composite material;
[0011] The aluminum alloy carbon fiber composite material comprises aluminum alloy, carbon fiber and a binder.
[0012] Furthermore, the aluminum alloy carbon fiber composite material comprises, by volume, 0.3% to 15% carbon fiber, 2.0% to 6.2% binder, and the remainder aluminum alloy.
[0013] Preferably, the noise-reducing and corrosion-resistant aluminum alloy product has a porosity of 75% to 90% and a pore size of 0.2 μm to 2 mm.
[0014] Preferably, the density of the noise-reducing and corrosion-resistant aluminum alloy product is 0.05 g / cm 3 ~0.8g / cm 3 .
[0015] Furthermore, the diameter of the carbon fiber is 0.01 nm to 5 μm.
[0016] Preferably, the tow specification of the carbon fiber is 12k-24k.
[0017] Preferably, the binder includes at least one of a polymer binder, a wax binder and a dextrin binder.
[0018] Preferably, the polymer binder comprises a resin binder.
[0019] Preferably, the aluminum alloy contains the following components: Cr 2.3wt.% to 6.5wt.%, Ni
[0020] 0.5wt.%~3.0wt.%, Mg 1.5wt.%~2.5wt.%, Si 0.4wt.%~2.0wt.%, and the balance is Al.
[0021] The second aspect of the present invention provides a process for preparing the noise-reducing and corrosion-resistant aluminum alloy product, comprising the following steps:
[0022] The aluminum alloy powder, carbon fiber and binder are granulated, the obtained granules are injection-molded to obtain green bodies, and the green bodies are degreased, sintered and extruded to obtain extruded wires of the composite material;
[0023] The extruded wires are woven into a mesh structure and then pressed into a desired shape and size to obtain the noise-reducing and corrosion-resistant aluminum alloy product.
[0024] Furthermore, in the granulation process, the mixing temperature is 130° C. to 150° C., and the mixing time is 45 min to 80 min.
[0025] Preferably, the particle size of the granules is ≤ 1 micron.
[0026] Preferably, in the injection molding, the mold temperature is 45-60° C., the injection temperature is 170-180° C., and the injection pressure is 115 MPa-135 MPa.
[0027] Furthermore, the degreasing includes two steps, firstly solvent degreasing and then thermal degreasing.
[0028] Preferably, the solvent used in the solvent degreasing is dichloromethane, and the temperature is 30°C to 50°C.
[0029] Preferably, the sintering temperature is 400° C. to 600° C., and the sintering time is 1 h to 5 h.
[0030] Furthermore, the sintered material is added into a twin-screw extruder, and the wire material is extruded through a die to obtain extruded wire.
[0031] Preferably, the diameter of the extruded filament is 0.01 mm-0.5 mm.
[0032] Furthermore, the method for preparing the aluminum alloy powder comprises the following steps:
[0033] The raw materials are added according to a proportion, then smelted and melted, and finally powdered to obtain the aluminum alloy powder.
[0034] Preferably, the smelting and melting temperature is 650°C to 850°C.
[0035] Preferably, the powder making method is high-pressure water atomization powder making.
[0036] Preferably, the pressure of the high-pressure water atomization powder making is 50MPa to 100MPa.
[0037] The third aspect of the present invention provides the use of the noise-reducing and corrosion-resistant aluminum alloy product in the preparation of mufflers, shock absorbers or sound insulation equipment.
[0038] Compared with the prior art, the present invention has at least the following beneficial effects:
[0039] The noise-reducing and corrosion-resistant aluminum alloy product provided by the present invention uses a composite material as a substrate, and carbon fiber is added to the composite material, which improves the mechanical properties and corrosion resistance of the composite material and prolongs the life of the composite material. The density of the noise-reducing and corrosion-resistant aluminum alloy product made of the composite material is only 0.05g / cm 3 ~0.8g / cm 3 , and the density can be adjusted according to the requirements of the application, which improves the sound absorption performance, reduces the weight of the material, and reduces the cost of use.
[0040] The preparation process provided by the present invention first prepares the composite material into filaments and then weaves them into a mesh structure, thereby improving the sound absorption performance of the noise-reducing and corrosion-resistant aluminum alloy product. Moreover, the preparation method is process controllable and can produce noise-reducing and corrosion-resistant aluminum alloy products of various specifications according to different application requirements. The process has high flexibility and strong controllability.
[0041] The application of the noise-reducing and corrosion-resistant aluminum alloy product of the present invention in mufflers, shock absorbers or sound insulation equipment not only improves the performance of the above equipment, reduces the cost, but also promotes the development of downstream industries. DETAILED DESCRIPTION
[0042] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution in the embodiment of the present invention will be clearly and completely described below in combination with the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, but not all of the embodiments. The components of the embodiment of the present invention can be arranged and designed in various different configurations.
[0043] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0044] A first aspect of the present invention provides a noise-reducing and corrosion-resistant aluminum alloy product, which is obtained by weaving fiber filaments of a composite material into a mesh, and then pressing the mesh structure into a desired shape and size;
[0045] Wherein, the composite material is an aluminum alloy carbon fiber composite material;
[0046] The aluminum alloy carbon fiber composite material comprises aluminum alloy, carbon fiber and a binder.
[0047] The noise-reducing and corrosion-resistant aluminum alloy product provided by the present invention uses a composite material as a substrate, and carbon fiber is added to the composite material, which improves the mechanical properties and corrosion resistance of the composite material and prolongs the life of the composite material. The density of the noise-reducing and corrosion-resistant aluminum alloy product made of the composite material is only 0.05g / cm 3 ~0.8g / cm 3 , and the density can be adjusted according to the requirements of the application, which improves the sound absorption performance, reduces the weight of the material, and reduces the cost of use.
[0048] Furthermore, the aluminum alloy carbon fiber composite material comprises, by volume, 0.3% to 15% carbon fiber, 2.0% to 6.2% binder, and the remainder aluminum alloy.
[0049] Typically but not limiting, in the aluminum alloy carbon fiber composite material, the volume proportion of carbon fiber can be, for example, 0.3%, 1%, 3%, 5%, 7%, 9%, 11%, 13% or 15%, or any value in the range of 0.3% to 15%; the volume proportion of the binder can be, for example, 2.0%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5% or 6.2%, or any value in the range of 2.0% to 6.2%;
[0050] Preferably, the noise-reducing and corrosion-resistant aluminum alloy product has a porosity of 75% to 90% and a pore size of 0.2 micrometers to 2 mm.
[0051] Preferably, the density of the noise-reducing and corrosion-resistant aluminum alloy product is 0.05 g / cm 3 ~0.8g / cm 3 .
[0052] Furthermore, the diameter of the carbon fiber is 0.01 nm to 5 μm.
[0053] Typically but not limiting, the diameter of the carbon fiber can be, for example, 0.01 nm, 0.1 nm, 0.5 nm, 1 nm, 10 nm, 50 nm, 100 nm, 500 nm, 1 μm, 2 μm, 3 μm, 4 μm or 5 μm; it can also be any value within the range of 0.01 nm to 5 μm.
[0054] Preferably, the tow specification of the carbon fiber is 12k-24k.
[0055] 12k means that the carbon fiber includes 12,000 filaments in each tow, and similarly, 24k means that the carbon fiber includes 24,000 filaments in each tow.
[0056] Preferably, the binder includes at least one of a polymer binder, a wax binder and a dextrin binder.
[0057] Preferably, the polymer binder comprises a resin binder.
[0058] Preferably, the aluminum alloy contains the following components: Cr 2.3wt.% to 6.5wt.%, Ni
[0059] 0.5wt.%~3.0wt.%, Mg 1.5wt.%~2.5wt.%, Si 0.4wt.%~2.0wt.%, and the balance is Al.
[0060] Typically but not limiting, in the aluminum alloy, the mass percentage of Cr is 2.3%, 2.8%, 3.2%, 3.7%, 4.1%, 4.6%, 5.1%, 5.8% or 6.5%, and can be any value in the range of 2.3wt.% to 6.5wt.%; the mass percentage of Ni is 0.5%, 1%, 1.5%, 2% or 3%, and can be any value in the range of 0.5wt.% to 3.0wt.%; the mass percentage of Mg is 1.5%, 1.7%, 1.9%, 2.1%, 2.3%, 2.4% or 2.5%, and can be any value in the range of 1.5wt.% to 2.5wt.%; the mass percentage of Si is 0.4%, 0.8%, 1.2%, 1.6% or 2.0%, and can be any value in the range of 0.4wt.% to 2.0wt.%.
[0061] The second aspect of the present invention provides a process for preparing the noise-reducing and corrosion-resistant aluminum alloy product, comprising the following steps:
[0062] The aluminum alloy powder, carbon fiber and binder are granulated, the obtained granules are injection-molded to obtain green bodies, and the green bodies are degreased, sintered and extruded to obtain extruded wires of the composite material;
[0063] The extruded wires are woven into a mesh structure and then pressed into a desired shape and size to obtain the noise-reducing and corrosion-resistant aluminum alloy product.
[0064] The preparation process provided by the present invention first prepares the composite material into filaments and then weaves them into a mesh structure. When sound waves pass through the mesh structure, they experience multiple reflections and scatterings, which increases the loss of sound wave energy and improves the sound absorption performance of the noise-reducing and corrosion-resistant aluminum alloy product. Moreover, the preparation method is process controllable and can produce noise-reducing and corrosion-resistant aluminum alloy products of various specifications according to different application requirements. The process has high flexibility and strong controllability.
[0065] Furthermore, in the granulation process, the mixing temperature is 130° C. to 150° C., and the mixing time is 45 min to 80 min.
[0066] Preferably, the particle size of the granules is ≤ 1 micron.
[0067] Preferably, in the injection molding, the mold temperature is 45-60° C., the injection temperature is 170-180° C., and the injection pressure is 115 MPa-135 MPa.
[0068] Furthermore, the degreasing includes two steps, firstly solvent degreasing and then thermal degreasing.
[0069] Preferably, the solvent used in the solvent degreasing is dichloromethane, and the temperature is 30°C to 50°C.
[0070] Preferably, the sintering temperature is 400° C. to 600° C., and the sintering time is 1 h to 5 h.
[0071] Furthermore, the sintered material is added into a twin-screw extruder, and the wire material is extruded through a die to obtain extruded wire.
[0072] Preferably, the diameter of the extruded filament is 0.01 mm-0.5 mm.
[0073] The diameter of the extruded filament is in the range of 0.01 mm-0.5 mm, which has better controllability and higher production efficiency. Typically but not limiting, the diameter of the extruded filament can be, for example, 0.01 mm, 0.05 mm, 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm or 0.5 mm, or any value in the range of 0.01 mm-0.5 mm.
[0074] The metal fibers are unidirectionally linked and woven into a mesh by a weaving device to obtain a primary metal fiber mesh, and the primary metal fiber mesh is stretched by a tensile testing machine to obtain a pretreated metal fiber mesh.
[0075] Repeat the operation to obtain a plurality of pre-treated metal fiber meshes. Furthermore, the method for preparing the aluminum alloy powder comprises the following steps:
[0076] The raw materials are added according to a proportion, then smelted and melted, and finally powdered to obtain the aluminum alloy powder.
[0077] It should be noted that the raw material here can be a single metal or in the form of an alloy.
[0078] Preferably, the smelting and melting temperature is 650°C to 850°C.
[0079] Typically but not limiting, the smelting and melting temperature may be, for example, 650°C, 700°C, 750°C, 800°C or 850°C, or any value within the range of 650°C to 850°C.
[0080] Preferably, the powder making method is high-pressure water atomization powder making.
[0081] High-pressure water atomization is a method of preparing aluminum alloy powder by using high-pressure water flow to melt aluminum alloy and then spray it into fine particles, and then quickly cool and solidify it. In the high-pressure water atomization process, the aluminum alloy is first heated to a molten state, and then sprayed into fine particles by high-pressure water flow. These particles form spherical powders during the process of rapid cooling and solidification.
[0082] Preferably, the pressure of the high-pressure water atomization powder making is 50MPa to 100MPa.
[0083] Typically but not restrictively, the pressure of high-pressure water atomization powder making can be, for example, 50 MPa, 60 MPa, 70 MPa, 80 MPa, 90 MPa or 100 MPa, or any value within the range of 50 MPa to 100 MPa.
[0084] The third aspect of the present invention provides the use of the noise-reducing and corrosion-resistant aluminum alloy product in the preparation of mufflers, shock absorbers or sound insulation equipment.
[0085] The application of the noise-reducing and corrosion-resistant aluminum alloy product of the present invention in mufflers, shock absorbers or sound insulation equipment not only improves the performance of the above equipment, reduces costs, but also promotes the development of downstream industries.
[0086] In the following, some embodiments of the present invention are described in detail in conjunction with the embodiments. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.
[0087] Example 1
[0088] A noise-reducing and corrosion-resistant aluminum alloy product, composed of an aluminum alloy, a carbon fiber reinforcement phase and a binder, wherein the volume percentage of the aluminum alloy is 91%, the volume percentage of the carbon fiber is 5.8%, and the volume percentage of the binder is 3.2%. The aluminum alloy is used as the main phase of the noise reduction material, and its components include: Cr 3.6wt.%, Ni 0.6wt.%, Si 1.1wt.%, Mg 1.8wt.%, and the balance is Al. The D50 diameter of the carbon fiber is 1 micron, a 20K tow is selected, and the binder is dichloromethane.
[0089] The preparation process of the noise-reducing and corrosion-resistant aluminum alloy product is as follows:
[0090] Aluminum and other added elements are smelted and melted in a suspension smelting furnace according to the corresponding proportions, the smelting temperature is 680℃, and then high-pressure water atomization powder is made under a pressure of 70MPa. The alloy powder and short carbon fiber are combined with a binder, and the feed is granulated. The mixing temperature during the granulation process is 140℃ and the mixing time is 45min. The particle size of the granules is 0.1 micron; the obtained granules are formed into green billets by injection molding, the injection temperature is 175℃, the injection pressure is 120MPa, and then thermal degreasing is carried out in an inert gas atmosphere. The degreased billets are sintered under the protection of an inert atmosphere. The solvent used in solvent degreasing is dichloromethane, the temperature is 35℃, the sintering temperature is 450℃, the time is 2.5h, and then cooled to room temperature. The obtained sintered green body is processed and extruded, the diameter of the extruded wire is 0.1mm, the metal wire is woven into a mesh structure, and different mesh sheets are pressed to finally form a multi-layer porous metal material. The product is processed into different shapes according to different needs.
[0091] Example 2
[0092] A noise reduction and corrosion resistant aluminum alloy product is only composed of aluminum alloy, wherein the volume percentage of the aluminum alloy is 100%. The aluminum alloy is used as the main phase of the noise reduction material, and its components include: Cr 4.5wt.%, Ni 1.5wt.%, Si2wt.%, Mg 2.0wt.%, and the balance is Al.
[0093] The preparation process is the same as that of Example 1.
[0094] Example 3
[0095] A noise-reducing and corrosion-resistant aluminum alloy product is composed of an aluminum alloy, a carbon fiber reinforcement phase, and a binder, wherein the volume percentage of the aluminum alloy is 95%, the volume percentage of the carbon fiber is 2.5%, and the volume percentage of the binder is 2.5%. The aluminum alloy is used as the main phase of the noise reduction material, and its components include: Cr6.5wt.%, Ni 1.8wt.%, Si 0.9wt.%, Mg 1.7wt.%, and the balance is Al. The D50 diameter of the carbon fiber is 1 micron, a 20K tow is selected, and dichloromethane is used as the binder.
[0096] The preparation process is the same as that of Example 1.
[0097] Example 4
[0098] A noise-reducing and corrosion-resistant aluminum alloy product, composed of an aluminum alloy, a carbon fiber reinforcement phase and a binder, wherein the volume percentage of the aluminum alloy is 85%, the volume percentage of the carbon fiber is 10%, and the volume percentage of the binder is 5%. The aluminum alloy is used as the main phase of the noise reduction material, and its components include: Cr 2.7wt.%, Ni 1.0wt.%, Si 1.8wt.%, Mg 2.3wt.%, and the balance is Al. The D50 diameter of the carbon fiber is 1 micron, a 20K tow is selected, and dichloromethane is used as the binder.
[0099] The preparation process is the same as that of Example 1.
[0100] Example 5
[0101] A noise-reducing and corrosion-resistant aluminum alloy product is composed of an aluminum alloy, a carbon fiber reinforcement phase, and a binder, wherein the volume percentage of the aluminum alloy is 87%, the volume percentage of the carbon fiber is 12%, and the volume percentage of the binder is 1%. The aluminum alloy is used as the main phase of the noise reduction material, and its components include: Cr 4.0wt.%, Ni 2.3wt.%, Si 1.5wt.%, Mg 1.2wt.%, and the balance is Al. The D50 diameter of the carbon fiber is 1 micron, a 20K tow is selected, and dichloromethane is used as the binder.
[0102] The preparation process is the same as that of Example 1.
[0103] Example 6
[0104] A noise-reducing and corrosion-resistant aluminum alloy product, composed of an aluminum alloy, a carbon fiber reinforcement phase, and a binder, wherein the volume percentage of the aluminum alloy is 97%, the volume percentage of the carbon fiber is 1%, and the volume percentage of the binder is 2%. The aluminum alloy is used as the main phase of the noise reduction material, and its components include: Cr 2.5wt.%, Ni 1.4wt.%, Si 1.3wt.%, Mg 2.5wt.%, and the balance is Al. The D50 diameter of the carbon fiber is 1 micron, a 20K tow is selected, and dichloromethane is used as the binder.
[0105] The preparation process is the same as that of Example 1.
[0106] Example 7
[0107] A noise-reducing and corrosion-resistant aluminum alloy product, composed of an aluminum alloy, a carbon fiber reinforcement phase and a binder, wherein the volume percentage of the aluminum alloy is 93%, the volume percentage of the carbon fiber is 3%, and the volume percentage of the binder is 4%. The aluminum alloy is used as the main phase of the noise reduction material, and its components include: Cr 3.0wt.%, Ni 0.9wt.%, Si 1.7wt.%, Mg 1.5wt.%, and the balance is Al. The D50 diameter of the carbon fiber is 1 micron, a 20K tow is selected, and dichloromethane is used as the binder.
[0108] The preparation process is the same as that of Example 1.
[0109] Example 8
[0110] A noise-reducing and corrosion-resistant aluminum alloy product is composed of an aluminum alloy, a carbon fiber reinforcement phase, and a binder, wherein the volume percentage of the aluminum alloy is 88%, the volume percentage of the carbon fiber is 10.5%, and the volume percentage of the binder is 1.5%. The aluminum alloy is used as the main phase of the noise reduction material, and its components include: Cr 6.0wt.%, Ni 2.8wt.%, Si 1.2wt.%, Mg 1.9wt.%, and the balance is Al. The D50 diameter of the carbon fiber is 1 micron, a 20K tow is selected, and dichloromethane is used as the binder.
[0111] The preparation process is the same as that of Example 1.
[0112] Comparative Example 1
[0113] This comparative example provides a polyurethane foam material with an open-cell structure, the characteristics of which are shown in Table 1 below.
[0114] Table 1
[0115]
[0116]
[0117] Test Example 1
[0118] The materials obtained in the examples and comparative examples were subjected to performance tests, specifically including alkali resistance, high temperature resistance, and sound absorption coefficient, and the obtained data are shown in Table 2 below.
[0119] The alkali resistance is tested in accordance with GB / T 32095.3-2015 "Performance and test specifications for non-stick surfaces of metal cooking utensils for household food Part 3: Corrosion resistance test specification".
[0120] High temperature performance is tested using the metal melting method.
[0121] The sound absorption coefficient is tested in a laboratory with corresponding qualifications.
[0122] Table 2
[0123] Alkali resistance High temperature resistance Sound absorption coefficient Example 1 No surface changes 425 0.71 Example 2 No surface changes 370 0.60 Example 3 No surface changes 410 0.69 Example 4 No surface changes 400 0.70 Example 5 No surface changes 470 0.75 Example 6 No surface changes 405 0.68 Example 7 No surface changes 420 0.72 Example 8 No surface changes 430 0.71 Comparative Example 1 Spots on the surface <100 0.7
[0124] It can be seen from Table 2 that excessive Al content will affect the alkali resistance and high temperature resistance of the material, making the value low; carbon fiber can increase the use temperature of the material, and the loose structure of carbon fiber can improve the noise reduction performance of the material. The four elements Cr, Ni, Si, and Mg can form solid solution phases or some special crystal structures according to different proportions to improve the density of the composite material.
[0125] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A noise-reducing and corrosion-resistant aluminum alloy product, characterized in that: Weaving the fiber filaments of the composite material into a mesh, and then pressing the mesh structure into a desired shape and size to obtain the noise-reducing and corrosion-resistant aluminum alloy product; Wherein, the composite material is an aluminum alloy carbon fiber composite material; The aluminum alloy carbon fiber composite material comprises aluminum alloy, carbon fiber and a binder.
2. The noise-reducing and corrosion-resistant aluminum alloy product according to claim 1, characterized in that: The aluminum alloy carbon fiber composite material comprises, by volume, 0.3% to 15% carbon fiber, 2.0% to 6.2% binder, and the remainder is aluminum alloy; Preferably, the porosity of the noise-reducing and corrosion-resistant aluminum alloy product is 75% to 90%, and the pore size is 0.2 μm to 2 mm; Preferably, the density of the noise-reducing and corrosion-resistant aluminum alloy product is 0.05 g / cm 3 ~0.8g / cm 3 .
3. The noise-reducing and corrosion-resistant aluminum alloy product according to claim 1 or 2, characterized in that: The diameter of the carbon fiber is 0.01nm to 5μm; Preferably, the tow specification of the carbon fiber is 12k to 24k; Preferably, the binder comprises at least one of a polymer binder, a wax binder and a dextrin binder; Preferably, the polymer binder comprises a resin binder; Preferably, the aluminum alloy contains the following components: Cr 2.3wt.% to 6.5wt.%, Ni 0.5wt.%~3.0wt.%, Mg 1.5wt.%~2.5wt.%, Si 0.4wt.%~2.0wt.%, and the balance is Al.
4. A process for preparing a noise-reducing and corrosion-resistant aluminum alloy product according to any one of claims 1 to 3, characterized in that: The following steps are involved: The aluminum alloy powder, carbon fiber and binder are granulated, the obtained granules are injection-molded to obtain green bodies, and the green bodies are degreased, sintered and extruded to obtain extruded wires of the composite material; The extruded wires are woven into a mesh structure and then pressed into a desired shape and size to obtain the noise-reducing and corrosion-resistant aluminum alloy product.
5. The preparation process according to claim 4, characterized in that: The mixing temperature in the granulation process is 130°C to 150°C, and the mixing time is 45min to 80min; Preferably, the particle size of the granules is ≤1 micron; Preferably, in the injection molding, the mold temperature is 45-60° C., the injection temperature is 170-180° C., and the injection pressure is 115 MPa-135 MPa.
6. The preparation process according to claim 4, characterized in that: The degreasing comprises two steps, firstly solvent degreasing and then thermal degreasing; Preferably, the solvent used in the solvent degreasing is dichloromethane, and the temperature is 30°C to 50°C; Preferably, the sintering temperature is 400° C. to 600° C., and the sintering time is 1 h to 5 h.
7. The preparation process according to claim 4, characterized in that: The sintered material is added into a twin-screw extruder, and the wire material is extruded through a die to obtain an extruded wire; Preferably, the diameter of the extruded filament is 0.01 mm-0.5 mm.
8. The preparation process according to any one of claims 4 to 7, characterized in that: The method for preparing the aluminum alloy powder comprises the following steps: The raw materials are fed according to a proportion, then smelted and melted, and finally powdered to obtain the aluminum alloy powder; Preferably, the smelting and melting temperature is 650°C to 850°C; Preferably, the powder making method is high-pressure water atomization powder making; Preferably, the pressure of the high-pressure water atomization powder making is 50MPa to 100MPa.
9. Use of the noise-reducing and corrosion-resistant aluminum alloy product according to any one of claims 1 to 5 in the preparation of mufflers, shock absorbers or sound insulation equipment.