Heat treatment method for ultrahigh-toughness gamma-TiAl intermetallic compound binary structure

Through solid solution treatment, multi-stage annealing and aging treatment, the microstructure of TiAl intermetallic compounds is regulated, and the problems of coarse tissue and poor toughness caused by traditional heat treatment are solved, and the two-state tissue that matches high strength and high toughness is achieved, suitable for aviation High temperature materials in the aerospace field.

CN118957463APending Publication Date: 2024-11-15ANSTEEL BEIJING RES INST CO LTD +2
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410746531.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The traditional TiAl intermetallic compound titanium alloy heat treatment process leads to large microstructure and large pitch of γ-phase layer sheets, resulting in poor plasticity and fracture toughness of the alloy, making it difficult to meet the requirements of high strength, high toughness and high temperature performance in the aerospace field.

Method used

The two-state tissue heat treatment method of ultra-high strength γ-TiAl intermetallic compound is adopted, and the ratio and grain size of the α2 phase and the γ phase are regulated through solid solution treatment, multi-stage annealing treatment and aging treatment to form a reasonable microstructure structure. Specific steps include solid solution treatment, primary annealing treatment, secondary annealing treatment and aging treatment, controlling temperature and time, and optimizing the size and distribution of γ grains and α2 grains.

Benefits of technology

The tensile strength, yield strength and elongation of TiAl intermetallic compounds are significantly improved, ensuring that their comprehensive mechanical properties at room temperature and high temperature are good, and matched with strong plasticity, and are suitable for high-temperature structural materials in the aerospace field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957463A_ABST
    Figure CN118957463A_ABST
Patent Text Reader

Abstract

The invention relates to a heat treatment method for a super-high-toughness gamma-TiAl intermetallic compound double-state structure. The heat treatment method comprises the steps of solution treatment, multi-stage annealing treatment and aging treatment. The method comprises the following steps: 1, solution treatment: heating a TiAl intermetallic compound to 20-120 DEG C above T beta, preserving heat for 30-60 minutes, and cooling to room temperature by water cooling; 2, primary annealing treatment is conducted, specifically, the TiAl intermetallic compound is heated to the temperature 50-100 DEG C higher than T alpha + beta, heat preservation is conducted for 1-2 h, and then the TiAl intermetallic compound is cooled to the room temperature; 3, secondary annealing treatment is conducted, specifically, the material obtained after cooling in the step 2 is heated to 100-150 DEG C below T alpha + beta along with the furnace, heat preservation is conducted for 1-2 h, and then water cooling is conducted to the room temperature; and fourthly, aging treatment is conducted, specifically, the material obtained after cooling in the third step is heated to 450-550 DEG C along with the furnace, heat preservation is conducted for 6-8 h, and then air cooling is conducted to the room temperature. According to the heat treatment technology, it can be guaranteed that the ratio of an alpha-phase structure to a gamma-phase structure is adjusted, the lamellar spacing is smaller after solution treatment, multi-stage annealing treatment and aging treatment, and the grain size is refined.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of high-temperature titanium alloy heat treatment technology, and in particular to a heat treatment method for a dual-state microstructure of ultra-high strength and toughness γ-TiAl intermetallic compounds. Background Art

[0002] With the development of aerospace technology, the increased speed and performance of weapons and equipment have placed higher demands on high-temperature structural materials. This requires the development of materials with high strength, high toughness, high specific strength, and excellent high-temperature performance, as well as forming technologies for their structural components. In order to meet the requirements of the rapid development of aerospace, it is urgent to develop new high-strength, high-toughness, TiAl intermetallic compound-resistant high-temperature titanium alloys and their corresponding heat treatment processes.

[0003] Heat treatment is one of the main methods for regulating the properties of high-strength and high-toughness titanium alloys. Traditional heat treatment of TiAl intermetallic compound titanium alloys mainly involves solution treatment followed by aging. After heat treatment, by controlling changes in the microstructure, their mechanical properties can be significantly altered. The morphology, content, and size of the main strengthening phases in the matrix have a crucial impact on the alloy's mechanical properties. Solution treatment is primarily used to obtain the metastable β phase. During aging, the metastable β phase decomposes, forming a large number of fine, dispersed age-aged α phases to strengthen the alloy. The strength and toughness of high-strength and high-toughness titanium alloys strongly depend on the morphology, quantity, and size of the age-aged α phase, while the transformation of the age-aged α phase into a smaller interlamellar spacing and smaller grain size depends on the aging temperature.

[0004] Typical heat treatment processes involve solution treatment in the single-phase region above the phase transformation point or the bidirectional region below the phase transformation point. For TiAl intermetallic compounds, after conventional heat treatment, the α-grains in the microstructure are relatively large and dispersed in the matrix, while the γ-phase lamellar spacing is large and their proportion is small. This results in poor plasticity and fracture toughness in the alloy after solution treatment and aging. Therefore, based on the commonly used solution treatment and aging process, it is of great significance to develop a suitable heat treatment process that comprehensively considers multiple influencing factors such as temperature, time, and the number of aging cycles to control the microstructure characteristics such as morphology, quantity, and size. This process can further improve the high strength of TiAl intermetallic compound titanium alloys while ensuring that the alloy's plasticity and toughness meet the requirements for service applications. Summary of the Invention

[0005] The technical problem to be solved by the present invention is to provide a heat treatment method for ultra-high strength and toughness γ-TiAl intermetallic compound dual-state microstructure, which can effectively control the microstructure to obtain a reasonable ratio of α2 phase and γ phase combination microstructure, and can ensure that the comprehensive mechanical properties and strength and plasticity at room temperature and high temperature are well matched.

[0006] To achieve the above objectives, the present invention employs the following technical solution:

[0007] A heat treatment method for ultra-high strength and toughness γ-TiAl intermetallic compound dual-state microstructure, consisting of solution treatment + multi-stage annealing + aging heat treatment;

[0008] Step 1: Solution treatment

[0009] The TiAl intermetallic compound was heated to T. β After maintaining the temperature at 20℃~120℃ for 30min~60min, cool to room temperature with water.

[0010] Step 2: Primary Annealing

[0011] The TiAl intermetallic compound was heated to T. α+β Keep at 50℃~100℃ for 1h~2h, then cool to room temperature;

[0012] Step 3: Secondary annealing

[0013] The material obtained after cooling in step two is heated to T in the furnace. α+β Keep warm at 100℃~150℃ for 1h~2h, then cool to room temperature with water;

[0014] Step 4: Time-sensitive processing

[0015] After cooling in step three, the material is heated in the furnace to 450℃~550℃ and held for 6-8 hours, then air-cooled to room temperature.

[0016] The TiAl intermetallic compound comprises, by atomic percentage, 43%–46% Al; 3%–5% Nb; 1%–2% Mo; 0.5%–0.8% C; 0.5%–0.8% B, with the balance being Ti and unavoidable impurities.

[0017] The solution treatment in step one is as follows: heating the TiAl intermetallic compound to T β Hold at 70℃~90℃ for 30min~60min, then cool to room temperature with water.

[0018] The first-stage annealing process in step two is as follows: heating the material cooled in step one to T. α+β Keep warm at 60℃~90℃ for 1h~2h; then air cool to room temperature.

[0019] The secondary annealing process in step three is as follows: the material cooled in step two is heated in the furnace to T. α+β Keep warm at 110℃~140℃ for 1h~2h; then cool to room temperature with water.

[0020] The aging treatment in step four is as follows: the material obtained after cooling in step three is heated to 495℃~505℃ in the furnace and held for 6h~8h, and then air-cooled to room temperature.

[0021] The performance indicators of an ultra-high strength and toughness γ-TiAl intermetallic compound are: tensile strength ≥1180MPa, yield strength ≥1060MPa, and elongation ≥6.0%.

[0022] Compared with existing technologies, the beneficial effects of this invention are:

[0023] This invention, employing a solution treatment + multi-stage annealing + aging treatment approach, compared to traditional heat treatment methods, achieves its advantages. By carefully selecting the holding temperature, holding time, and cooling method during multi-stage annealing, the solution treatment effectively controls the microstructure, resulting in microstructures with varying proportions of α2 and γ phases. The multi-stage annealing further optimizes the grain size of γ and α2 phases and enhances the solidification ability of the microstructure, thereby obtaining an ideal dual-state microstructure. This results in γ-TiAl high-temperature titanium alloys exhibiting higher strength and better toughness at both room temperature and high temperature. The products obtained by this invention exhibit excellent performance, and the process is simple and easy to control, facilitating large-scale industrial production.

[0024] The present invention provides a heat treatment method for the dual-state structure of ultra-high strength and toughness γ-TiAl intermetallic compounds. After the first step of the solution treatment, the γ phase in the α2 phase is fully and uniformly decomposed, which facilitates the subsequent heat treatment process to re-precipitate fine and uniformly distributed γ phase, and at the same time eliminates the stress generated by rolling.

[0025] After the second step of primary annealing, the microstructure consists of a large proportion of α2 phase with large grain size and γ phase with large interlamellar spacing. The γ lamellars occupy a relatively small proportion, with a volume fraction of only 20%, and are large in size, with an average grain size of about 20 μm. The α2 phase grain size is about 45 μm.

[0026] After the third step of secondary annealing, the grain size of the α2 phase is refined to an average size of about 10 μm. The proportion of lamellar clusters of the γ phase increases, the spacing between the clusters decreases, and the grain size is further refined to about 5 μm.

[0027] After the fourth step of aging treatment, the microstructure is cooled to room temperature. The microstructure is a bimodal structure of α2 and γ phases, with the ratio of the two phases being close to 1:1. The spacing between the γ crystal clusters is relatively small, with a volume fraction of about 45%, while the volume fraction of α2 is about 55%.

[0028] The solution treatment, multi-stage annealing, and aging treatment of this invention first select the phase transformation point T. β Perform a solution treatment at a slightly higher temperature, and then at T α+β The above undergoes a first-stage annealing process, followed by T... α+β The next step is to perform secondary annealing.

[0029] This heat treatment process not only ensures the adjustment of the ratio between the α-phase and γ-phase structures, but also achieves a smaller interlamellar spacing and effectively refines the grain size. Compared with existing processes, the grain size is significantly reduced by 5μm to 10μm, and the ratio between the α-phase and γ-phase structures changes from 1:0.75 to nearly 1:1, resulting in higher overall mechanical properties for the TiAl intermetallic compound.

[0030] In this invention, a solution treatment followed by multi-stage annealing and aging is performed, with the first solution treatment temperature controlled at T. β The temperature is maintained at 20℃~120℃ for 30min~60min to ensure the full and uniform decomposition of the γ phase within the α2 phase in the original microstructure, while simultaneously eliminating the stress generated during rolling; the first annealing temperature T is controlled. α+β After holding at 50℃~100℃ for 1h~2h, due to the relatively dense distribution of the α phase in the original microstructure, if the temperature is too low, the lamellar structure of the γ phase after solution treatment will be less and the interlamellar spacing will be larger; moreover, the volume difference between the two phases will be large, and if the temperature is too high, the material will be overburned, and the microstructure will be too coarse, reaching the millimeter level, which will adversely affect the mechanical properties after subsequent treatment; control the second annealing temperature T α+β After holding at 100℃~150℃ for 1h~2h, the grains are further refined, and the interlamellar spacing is reduced. After aging treatment, the microstructure is a bimodal structure of α2 and γ phases, with a ratio close to 1:1. The γ clusters have a smaller spacing, which has a significant impact on the yield strength and elongation of the alloy, thus adjusting the overall mechanical properties. Effective control of the microstructure to obtain a reasonable ratio of α2 and γ phases ensures a good match between its comprehensive mechanical properties and strength and ductility at both room temperature and high temperature, making it valuable for industrial applications.

[0031] The heat treatment process of this invention is simple, and the treated TiAl intermetallic compound exhibits good comprehensive mechanical properties such as tensile strength, yield strength, and elongation, making it an effective means to improve the strength and plasticity of TiAl intermetallic compounds. As can be seen from the examples and comparative data, this invention further improves the plasticity and elongation of TiAl intermetallic compounds while ensuring good strength, and the process is significantly superior to traditional heat treatment methods, thus giving it industrial application value. Attached Figure Description

[0032] Appendix Figure 1 This is a microscopic morphology image of the TiAl intermetallic compound after processing according to Example 1 of the present invention.

[0033] Appendix Figure 2 This is a microscopic morphology image of the TiAl intermetallic compound after processing according to Example 2 of the present invention.

[0034] Appendix Figure 3 This is a microscopic morphology image of the TiAl intermetallic compound after primary annealing and air cooling in Example 1 of the present invention.

[0035] Appendix Figure 4 This is a microscopic morphology image of the TiAl intermetallic compound after secondary annealing and water cooling in Example 1 of the present invention. Detailed Implementation

[0036] It should be noted that, unless otherwise specified, the embodiments and features described in the present invention can be combined with each other.

[0037] In the description of this invention, it should be understood that the terms "center," "longitudinal," "lateral," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," and "outer," etc., indicating orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, are used only for the convenience of describing the invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of the invention. Furthermore, the terms "first," "second," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, a feature defined with "first," "second," etc., may explicitly or implicitly include one or more of that feature. In the description of this invention, unless otherwise stated, "a plurality of" means two or more.

[0038] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art will understand the specific meaning of the above terms in this invention based on the specific circumstances.

[0039] A heat treatment method for ultra-high strength and toughness γ-TiAl intermetallic compound dual-state microstructure, the heat treatment is solution treatment + multi-stage annealing treatment + aging heat treatment;

[0040] Step 1: Solution treatment, heating the TiAl intermetallic compound to T β After maintaining the temperature at 20℃~120℃ for 30min~60min, cool to room temperature with water.

[0041] Step 2: Primary annealing treatment, heating the TiAl intermetallic compound to T α+β Keep at 50℃~100℃ for 1h~2h, then cool to room temperature;

[0042] Step 3: Secondary annealing treatment. The material obtained after cooling in Step 2 is heated in the furnace to T. α+β Keep warm at 100℃~150℃ for 1h~2h, then cool to room temperature with water;

[0043] Step 4: Aging treatment. After cooling in Step 3, heat the material in the furnace to 450℃~550℃ and hold for 6h~8h, then air cool to room temperature.

[0044] A heat treatment method for ultra-high strength and toughness γ-TiAl intermetallic compound dual-state microstructure, comprising solution treatment + multi-stage annealing + aging heat treatment; the product has a tensile strength of 1210MPa~1295MPa, a yield strength of 1110MPa~1168MPa, and an elongation of 6.0%~6.5%, specifically including:

[0045] Step 1: Solution treatment, heating the TiAl intermetallic compound to T β The temperature was maintained at 70℃~90℃ for 30 minutes, then cooled to room temperature with water.

[0046] Step 2: Primary annealing treatment, heating the TiAl intermetallic compound to T α+β Keep at 75℃~85℃ for 1 hour, then cool to room temperature;

[0047] Step 3: Secondary annealing treatment. The material obtained after cooling in Step 2 is heated in the furnace to T. α+β Keep warm at 125℃~135℃ for 1 hour, then cool to room temperature with water;

[0048] Step 4: Aging treatment. The material obtained after cooling in Step 3 is heated in the furnace to 495℃~505℃ and held for 6 hours, then air-cooled to room temperature.

[0049] A heat treatment method for ultra-high strength and toughness γ-TiAl intermetallic compound dual-state microstructure, comprising solution treatment + multi-stage annealing + aging heat treatment; the product achieves tensile strength of 1263 MPa–1341 MPa, yield strength of 1060 MPa–1132 MPa, and elongation of 5.7%–6.1%, specifically including:

[0050] Step 1: Solution treatment, heating the TiAl intermetallic compound to T β The temperature was maintained at 55℃~65℃ for 30 minutes, then cooled to room temperature with water.

[0051] Step 2: Primary annealing treatment, heating the TiAl intermetallic compound to T α+β Keep at 65℃~75℃ for 1 hour, then cool to room temperature;

[0052] Step 3: Secondary annealing treatment. The material obtained after cooling in Step 2 is heated in the furnace to T. α+β Keep warm at 115℃~125℃ for 1 hour, then cool to room temperature with water;

[0053] Step 4: Aging treatment. The material obtained after cooling in Step 3 is heated in the furnace to 495℃~505℃ and held for 6 hours, then air-cooled to room temperature.

[0054] A heat treatment method for ultra-high strength and toughness γ-TiAl intermetallic compound dual-state microstructure, comprising solution treatment + multi-stage annealing + aging heat treatment; the product achieves tensile strength of 1222MPa~1298MPa, yield strength of 1143MPa~1205MPa, and elongation of 6.4%~7.3%, specifically including:

[0055] Step 1: Solution treatment, heating the TiAl intermetallic compound to T β After maintaining the temperature at 70℃ for 60 minutes, cool it down to room temperature with water.

[0056] Step 2: Primary annealing treatment, heating the TiAl intermetallic compound to T α+β Keep at 80℃ for 2 hours, then cool to room temperature;

[0057] Step 3: Secondary annealing treatment. The material obtained after cooling in Step 2 is heated in the furnace to T. α+β Keep at 120℃ for 1 hour, then cool to room temperature with water;

[0058] Step 4: Aging treatment. The material obtained after cooling in Step 3 is heated to 550℃ in the furnace and held for 6 hours, then air-cooled to room temperature.

[0059] The preferred embodiments of the present invention have been described in detail above with reference to the accompanying drawings. However, the present invention is not limited to the specific details of the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solutions of the present invention, and these simple modifications all fall within the protection scope of the present invention. Furthermore, it should be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, the present invention will not describe the various possible combinations separately. In addition, various different embodiments of the present invention can also be arbitrarily combined, as long as they do not violate the spirit of the present invention, and should also be considered as the content disclosed by the present invention.

[0060] To make the objectives, technical solutions, and technical effects of this invention clearer, the technical solutions in the embodiments of this invention are now described clearly and completely. However, the embodiments described below are only some embodiments of this invention, not all embodiments. All other embodiments obtained by those skilled in the art in conjunction with the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0061] Example

[0062] TiAl intermetallic compound sheets, by atomic percentage, comprise 43% Al; 3% Nb; 1% Mo; 0.5% C; 0.5% B, with the balance being Ti and unavoidable impurities. The manufacturing process for TiAl intermetallic compound sheets includes smelting, casting, rolling, and heat treatment. The β-phase transformation temperature of TiAl intermetallic compound sheets is 1280℃±5℃, and the α+β phase transformation point is 1080℃±5℃.

[0063] Example 1

[0064] A heat treatment method for ultra-high strength and toughness γ-TiAl intermetallic compound dual-state microstructure includes the following steps: 1) Heating a 6mm×100mm×200mm TiAl intermetallic compound sheet to 1330℃, holding for 30 min, and then water-cooling to room temperature; 2) Heating the cooled sheet to 1140℃ and holding for 1 h at a heating rate of 10℃ / min, followed by air cooling to room temperature; 3) Heating the sheet obtained in step 2) to 940℃ in a furnace and holding for 2 h at a heating rate of 10℃ / min, followed by water cooling to room temperature; 4) Heating the sheet obtained in step 3) to 495℃~505℃ in a furnace and holding for 6 h at a heating rate of 10℃ / min, followed by air cooling to room temperature. The resulting product has an average tensile strength of 1186MPa (maximum value up to 1192MPa), an average yield strength of 1062MPa (maximum value up to 1069MPa), and an average elongation of 6.02% (maximum value up to 6.11%).

[0065] After heat treatment, the TiAl intermetallic compound plates were pre-ground, polished, and etched. Their microstructure was observed using an electron microscope, and their mechanical properties were tested using a universal testing machine. Microscopic images of the TiAl intermetallic compounds are shown below. Figure 1 . Figure 1 As can be seen, the α2 phase is uniformly distributed with an average size of 10 μm to 12 μm, accounting for about 60%, while the γ phase has a larger interlamellar spacing, accounting for a smaller proportion, only 40%, with a size of 35 μm to 45 μm.

[0066] See after primary annealing Figure 3As can be seen, the α2 phase is uniformly distributed with an average size of 60μm to 100μm, accounting for about 84%. The interlamellar spacing of the γ phase is relatively large, with an average size of 35μm to 45μm. After primary annealing, the α2 grain size is relatively large, and the γ phase is a relatively coarse lamellar structure.

[0067] See after secondary annealing Figure 4 It can be seen that the grains of the α2 and γ phases in the matrix are refined, the interlamellar spacing of γ is very small, accounting for about 35%, and the average size is 4μm to 6μm.

[0068] The product obtained in Example 1 has an average tensile strength of 1186 MPa (maximum value up to 1192 MPa), an average yield strength of 1062 MPa (maximum value up to 1069 MPa), and an average elongation of 6.02% (maximum value up to 6.11%). The room temperature mechanical properties of the TiAl intermetallic compound are shown in Table 1.

[0069] Example 2:

[0070] A heat treatment method for ultra-high strength and toughness γ-TiAl intermetallic compound dual-state microstructure includes: 1) heating a 6mm×100mm×200mm TiAl intermetallic compound plate to 1370℃, holding it at that temperature for 30min, and then water-cooling it to room temperature; 2) heating the cooled plate to 1170℃ in the furnace and holding it at that temperature for 1h, with a heating rate of approximately 10℃ / min, and then air-cooling it to room temperature; 3) heating the cooled plate to 970℃ in the furnace and holding it at that temperature for 2h, with a heating rate of approximately 10℃ / min, and then water-cooling it to room temperature; 4) heating the cooled plate to 495℃~505℃ in the furnace and holding it at that temperature for 6h, with a heating rate of approximately 10℃ / min, and then air-cooling it to room temperature.

[0071] After heat treatment, the TiAl intermetallic compound samples were pre-ground, polished, and etched. Their microstructure was observed using an electron microscope, and their mechanical properties were tested using a universal testing machine. Microscopic images of the TiAl intermetallic compounds are shown below. Figure 2 . Figure 2 It can be seen that the α2 phase is uniformly distributed with an average size of 8μm to 10μm and accounts for about 55%. The interlamellar spacing of the γ tissue decreases, while its proportion increases to 45% with an average size of 4μm to 6μm.

[0072] The product obtained in Example 2 has an average tensile strength of 1195 MPa (maximum value up to 1202 MPa), an average yield strength of 1068 MPa (maximum value up to 1072 MPa), and an average elongation of 6.01% (maximum value up to 6.19%). The room temperature mechanical properties of the TiAl intermetallic compound from Example 2 are shown in Table 1.

[0073] Example 3:

[0074] A heat treatment method for ultra-high strength and toughness γ-TiAl intermetallic compound dual-state microstructure: 1) A 6mm×100mm×200mm TiAl intermetallic compound plate is heated to 1355℃, held for 60min, and then water-cooled to room temperature; 2) The cooled plate is heated in the furnace to 1160℃ and held for 1h at a heating rate of approximately 10℃ / min, and then air-cooled to room temperature; 3) The cooled plate is heated in the furnace to 950℃ and held for 2h at a heating rate of approximately 10℃ / min, and then water-cooled to room temperature; 4) The cooled material is heated in the furnace to 545℃~555℃ and held for 6h at a heating rate of approximately 10℃ / min, and then air-cooled to room temperature.

[0075] After heat treatment, the TiAl intermetallic compound samples were pre-ground, polished, and etched. The microstructure was observed using an electron microscope, and the mechanical properties were tested using a universal testing machine. The product obtained in Example 3 had an average tensile strength of 1255 MPa (maximum value up to 1289 MPa), an average yield strength of 1135 MPa (maximum up to 1160 MPa), and an average elongation of 6.32% (maximum up to 6.48%). The room temperature mechanical properties of the TiAl intermetallic compound treated in this example are shown in Table 1.

[0076] Example 4:

[0077] A heat treatment method for ultra-high strength and toughness γ-TiAl intermetallic compound dual-state microstructure: 1) A 6mm×100mm×200mm TiAl intermetallic compound plate is heated to 1355℃, held for 60min, and then water-cooled to room temperature; 2) The cooled plate is heated in the furnace to 1170℃ and held for 1h at a heating rate of approximately 10℃ / min, and then air-cooled to room temperature; 3) The cooled plate is heated in the furnace to 945℃ and held for 2h at a heating rate of approximately 10℃ / min, and then water-cooled to room temperature; 4) The cooled material is heated in the furnace to 495℃~505℃ and held for 6h at a heating rate of approximately 10℃ / min, and then air-cooled to room temperature.

[0078] After heat treatment, the TiAl intermetallic compound samples were pre-ground, polished, and etched. The microstructure was observed using an electron microscope, and the mechanical properties were tested using a universal testing machine. The product obtained in Example 4 had an average tensile strength of 1276 MPa (maximum 1295 MPa), an average yield strength of 1140 MPa (maximum 1167 MPa), and an average elongation of 6.46% (maximum 6.56%). The room temperature mechanical properties of the TiAl intermetallic compound treated in this example are shown in Table 1.

[0079] Example 5:

[0080] A heat treatment method for ultra-high strength and toughness γ-TiAl intermetallic compound dual-state microstructure involves heat treatment using a 6mm×100mm×200mm TiAl intermetallic compound sheet. The first step involves heating the alloy to 1345℃, holding it at that temperature for 60 minutes, and then water-cooling it to room temperature. The second step involves heating the sheet obtained in the first step to 1150℃ in the furnace and holding it for 1 hour at a heating rate of approximately 10℃ / min, followed by air cooling to room temperature. The third step involves heating the material obtained in the second step to 975℃ in the furnace and holding it for 2 hours at a heating rate of approximately 10℃ / min, followed by water cooling to room temperature. The fourth step involves heating the material obtained in the third step to 495℃~505℃ in the furnace and holding it for 6 hours at a heating rate of approximately 10℃ / min, followed by air cooling to room temperature.

[0081] After heat treatment, the TiAl intermetallic compound samples were pre-ground, polished, and etched. The microstructure was observed using an electron microscope, and the mechanical properties were tested using a universal testing machine. The product obtained in Example 5 had an average tensile strength of 1305 MPa (maximum 1330 MPa), an average yield strength of 1097 MPa (maximum 1108 MPa), and an average elongation of 5.89% (maximum 6.06%). The room temperature mechanical properties of the TiAl intermetallic compound treated in this example are shown in Table 1.

[0082] Example 6:

[0083] A heat treatment method for ultra-high strength and toughness γ-TiAl intermetallic compound dual-state microstructure includes: 1) heating a 6mm×100mm×200mm TiAl intermetallic compound plate to 1345℃, holding it at that temperature for 60min, and then water-cooling it to room temperature; 2) heating the cooled plate to 1155℃ in the furnace and holding it at that temperature for 1h, with a heating rate of approximately 10℃ / min, and then air-cooling it to room temperature; 3) heating the cooled plate to 950℃ in the furnace and holding it at that temperature for 2h, with a heating rate of approximately 10℃ / min, and then water-cooling it to room temperature; 4) heating the cooled material to 495℃~505℃ in the furnace and holding it at that temperature for 6h, with a heating rate of approximately 10℃ / min, and then air-cooling it to room temperature.

[0084] After heat treatment, the TiAl intermetallic compound samples were pre-ground, polished, and etched. The microstructure was observed using an electron microscope, and the mechanical properties were tested using a universal testing machine. The product obtained in Example 6 had an average tensile strength of 1289 MPa (maximum value up to 1315 MPa), an average yield strength of 1102 MPa (maximum up to 1126 MPa), and an average elongation of 5.94% (maximum up to 6.16%). The room temperature mechanical properties of the TiAl intermetallic compound treated in this example are shown in Table 1.

[0085] Example 7:

[0086] A heat treatment method for ultra-high strength and toughness γ-TiAl intermetallic compound dual-state microstructure includes: 1) heating a 6mm×100mm×200mm TiAl intermetallic compound plate to 1350℃, holding it at that temperature for 60min, and then water-cooling it to room temperature; 2) heating the cooled plate to 1160℃ in the furnace and holding it at that temperature for 2h at a heating rate of approximately 10℃ / min, and then air-cooling it to room temperature; 3) heating the cooled plate to 960℃ in the furnace and holding it at that temperature for 1h at a heating rate of approximately 10℃ / min, and then water-cooling it to room temperature; 4) heating the cooled material to 550℃ in the furnace and holding it at that temperature for 6h at a heating rate of approximately 10℃ / min, and then air-cooling it to room temperature.

[0087] After heat treatment, the TiAl intermetallic compound samples were pre-ground, polished, and etched. The microstructure was observed using an electron microscope, and the mechanical properties were tested using a universal testing machine. The product obtained in Example 7 had an average tensile strength of 1294 MPa (maximum 1298 MPa), an average yield strength of 1185 MPa (maximum 1205 MPa), and an average elongation of 7.15% (maximum 7.36%). The room temperature mechanical properties of the TiAl intermetallic compound treated in this example are shown in Table 1.

[0088] Comparative Example 1

[0089] Heat treatment was performed using a 6mm×100mm×200mm TiAl intermetallic compound plate. The first step involved heating the alloy to 1290℃, holding it for 30 minutes, and then water-cooling it to room temperature. The second step involved aging treatment: the material obtained after cooling in the first step was heated to 600℃ in the furnace and held for 6 hours at a heating rate of approximately 10℃ / min, and then water-cooled to room temperature.

[0090] After heat treatment, the TiAl intermetallic compound samples were pre-ground, polished, and etched. Their microstructure was observed using an electron microscope, and their mechanical properties were tested using a universal testing machine. The room temperature mechanical properties of the treated TiAl intermetallic compound in this embodiment are shown in Table 1.

[0091] Comparative Example 2

[0092] Heat treatment was performed using a 6mm×100mm×200mm TiAl intermetallic compound plate. The first step involved heating the alloy to 1290℃, holding it at that temperature for 60 minutes, and then water-cooling it to room temperature. The second step involved aging treatment: the material obtained after cooling in the first step was heated to 600℃ in the furnace and held at that temperature for 6 hours at a heating rate of approximately 10℃ / min, and then water-cooled to room temperature.

[0093] After heat treatment, the TiAl intermetallic compound samples were pre-ground, polished, and etched. Their microstructure was observed using an electron microscope, and their mechanical properties were tested using a universal testing machine. The room temperature mechanical properties of the treated TiAl intermetallic compound in this embodiment are shown in Table 1.

[0094] Comparative Example 3

[0095] Heat treatment was performed using a 6mm×100mm×200mm TiAl intermetallic compound plate. The first step involved heating the alloy to 1320℃, holding it at that temperature for 30 minutes, and then water-cooling it to room temperature. The second step involved aging treatment: the material obtained after cooling in the first step was loaded into the furnace when the furnace temperature reached 500℃, and then heated to 550℃ and held for 6 hours at a heating rate of approximately 10℃ / min. After that, it was water-cooled to room temperature.

[0096] After heat treatment, the TiAl intermetallic compound samples were pre-ground, polished, and etched. Their microstructure was observed using a scanning electron microscope, and their mechanical properties were tested using a universal testing machine. The room temperature mechanical properties of the treated TiAl intermetallic compounds in this embodiment are shown in Table 1.

[0097] Comparative Example 4

[0098] Heat treatment was performed using a 5mm×110mm×180mm TiAl intermetallic compound plate. The first step involved heating the alloy to 1320℃, holding it at that temperature for 60 minutes, and then water-cooling it to room temperature. The second step involved aging treatment: the material obtained after cooling in the first step was heated to 550℃ in the furnace and held at that temperature for 6 hours at a heating rate of approximately 10℃ / min, and then water-cooled to room temperature.

[0099] After heat treatment, the TiAl intermetallic compound samples were pre-ground, polished, and etched. Their microstructure was observed using an electron microscope, and their mechanical properties were tested using a universal testing machine. The room temperature mechanical properties of the treated TiAl intermetallic compound in this embodiment are shown in Table 1.

[0100] Table 1 Mechanical properties of TiAl intermetallic compounds obtained in the examples and comparative examples

[0101] Case Average tensile strength (MPa) Mean yield strength (MPa) Average elongation (%) Implementation 1 1186 1062 6.02 Implementation 2 1195 1068 6.01 Implementation 3 1255 1135 6.32 Implementation 4 1276 1140 6.46 Implementation 5 1305 1097 5.89 Implementation 6 1289 1102 5.94 Implementation 7 1098 1185 8.68 Comparison 1 978 789 3.12 Comparison 2 965 801 3.24 Comparison 3 921 856 4.16 Comparison 4 894 756 4.02

[0102] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A heat treatment method for dual-state structure of ultra-high strength and toughness γ-TiAl intermetallic compound, It is characterized in that Solution treatment + multi-stage annealing + aging heat treatment; Step 1: Solution treatment The TiAl intermetallic compound is heated to T β Above 20℃~120℃, keep warm for 30min~60min, then cool to room temperature with water; Step 2: Primary annealing The TiAl intermetallic compound is heated to T α+β Above 50℃~100℃, keep warm for 1h~2h, then cool to room temperature; Step 3: Secondary annealing The material obtained after cooling in step 2 is heated to T α+β Keep at 100℃~150℃ for 1h~2h, then cool to room temperature with water; Step 4: Aging Process The material obtained after cooling in step 3 is heated to 450°C-550°C in a furnace and kept at this temperature for 6-8 hours, and then air-cooled to room temperature. The TiAl intermetallic compound comprises, by atomic percentage, 43% to 46% Al, 3% to 5% Nb, 1% to 2% Mo, 0.5% to 0.8% C, 0.5% to 0.8% B, and the remainder is Ti and unavoidable impurities.

2. A heat treatment method for dual-state structure of ultra-high strength and toughness γ-TiAl intermetallic compound according to claim 1, It is characterized in that The solution treatment in step 1 is as follows: heating the TiAl intermetallic compound to T β Keep the temperature at 70℃~90℃ for 30min~60min, then cool to room temperature with water.

3. A heat treatment method for dual-state structure of ultra-high strength and toughness γ-TiAl intermetallic compound according to claim 1, It is characterized in that The primary annealing treatment in step 2 is as follows: heating the material cooled in step 1 to T α+β Keep at 60℃~90℃ for 1h~2h; then air cool to room temperature.

4. A heat treatment method for dual-state structure of ultra-high strength and toughness γ-TiAl intermetallic compound according to claim 1, It is characterized in that The secondary annealing treatment in step 3 is as follows: the material cooled in step 2 is heated to T α+β Keep at 110℃~140℃ for 1h~2h; then cool to room temperature with water.

5. A heat treatment method for dual-state structure of ultra-high strength and toughness γ-TiAl intermetallic compound according to claim 1, It is characterized in that The aging treatment in step 4 is as follows: the material obtained after cooling in step 3 is heated to 495°C to 505°C in a furnace and kept at this temperature for 6h to 8h, and then air-cooled to room temperature.

6. The ultra-high strength and toughness γ-TiAl intermetallic compound according to claim 1, It is characterized in that Performance indicators: tensile strength ≥1180MPa, yield strength ≥1060MPa, elongation ≥6.0%.

Citation Information

Cited By

  • Strengthening and toughening regulation and control method for multi-stage sequential TiAl single crystal

    CN119530985A

  • Method for strengthening and toughening of multi-stage ordered TiAl single crystal

    CN119530985B