High-strength hot-dip galvanized steel, preparation method and application of high-strength hot-dip galvanized steel in manufacturing of fasteners

By using low-carbon boron steel and optimized processes in hot-dip galvanized steel, a micro-decarbonized layer and a transition layer are formed, which solves the problem of insufficient interface bonding strength and corrosion resistance, and improves the comprehensive performance of hot-dip galvanized steel. An efficient and environmentally friendly preparation process has been achieved.

CN118957476AActive Publication Date: 2024-11-15LENGSHUIJIANG TIANBAO IND
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411444426.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-11-15
Estimated Expiration
2044-10-16

AI Technical Summary

Technical Problem

The existing hot-dip galvanized steel has shortcomings in interface combination strength, fastener strength and corrosion resistance, resulting in insufficient plating peeling, cracking and corrosion resistance, limiting its application range and service life.

Method used

Low-carbon boron steel is used as the substrate, and a micro-decarbonized layer is formed through step-heating quenching. The pre-treatment process and hot-dip galvanizing process are optimized, the transition layer and galvanized layer are introduced, and the thickness and composition of the transition layer are optimized to form high strength and high Corrosion-resistant hot-dip galvanized steel.

Benefits of technology

It significantly improves the interface combination strength between the plating and the substrate, the strength of the fastener and the corrosion resistance of the plating, reduces production costs, simplifies the process flow, and achieves energy-saving and environmentally friendly benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957476A_ABST
    Figure CN118957476A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of galvanized steel materials, and provides high-strength hot-dip galvanized steel, a preparation method and application of the high-strength hot-dip galvanized steel to manufacturing of fasteners. The preparation method comprises the following steps: S1, cleaning; s2, step heating and quenching treatment; s3, acid pickling, water washing and plating assisting treatment are sequentially carried out within 1 h after discharging; s4, hot-dip galvanizing is conducted, and then centrifugal dezincification, water cooling and discharging treatment are conducted in sequence; the hot-dip galvanized steel comprises a carbon steel layer, a transition layer and a galvanized layer, wherein the transition layer and the galvanized layer are located on the carbon steel layer. The transition layer comprises zeta-FeZn13, delta-FeZn10 and Fe2B. According to the method, the precisely-controlled stepped heating, quenching and hot-dip galvanizing processes are adopted, the excellent interface bonding strength and corrosion resistance are achieved, and the problem that the interface bonding strength of traditional hot-dip galvanized steel is insufficient is solved by forming a lattice matching interface and a special microstructure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of galvanized steel materials, and in particular to high-strength hot-dip galvanized steel, a preparation method and application thereof in manufacturing fasteners. Background Art

[0002] High-strength hot-dip galvanized fasteners play a vital role in modern industry and infrastructure construction. They are widely used in photovoltaic power generation, 5G communications, ultra-high voltage transmission lines, highway guardrails, and other fields, connecting and securing key components. These applications place stringent performance demands on fasteners, including high strength, excellent interfacial bonding strength, and outstanding corrosion resistance. High strength is a fundamental performance requirement for fasteners, determining their ability to provide reliable connections under complex stress conditions.

[0003] Taking photovoltaic power generation and ultra-high voltage transmission as examples, fasteners need to withstand static and dynamic combined stresses such as wind loads and ice loads for a long time, and the loads change frequently. Improving strength performance is crucial to ensuring the safety of key components. In applications such as highway guardrails, fasteners must also have sufficient toughness to avoid brittle fracture failure. Interface bonding strength is a key indicator for measuring the quality of the bond between the coating and the substrate of hot-dip galvanized fasteners. Excellent bonding strength is a prerequisite for the coating to play its corrosion-resistant role. It not only affects the service life of the fasteners, but also the reliability and safety of the entire structure. Taking 5G communication base stations as an example, their fasteners are directly exposed to the atmospheric environment. Good bonding strength can prevent the coating from failing due to shedding, cracking, and other failures under wind and sun, thereby maximizing its service life and reducing maintenance and replacement costs. Corrosion resistance is the core advantage of hot-dip galvanized fasteners and plays an indispensable role in extending the life of fasteners and ensuring the safety of connection structures.

[0004] As we all know, steel is highly susceptible to electrochemical corrosion, and the volume expansion of its corrosion products can also lead to stress corrosion cracking. The hot-dip galvanizing process forms a dense zinc coating and zinc-iron alloy layer on the surface of fasteners, leveraging the coating's cathodic protection and insulation properties to significantly improve the fasteners' corrosion resistance. For example, offshore wind turbine fasteners operate in harsh environments with high salt spray concentrations. Continuously improving the corrosion resistance of the coating is crucial to ensuring the safe operation of wind turbines and extending their service life.

[0005] In summary, high strength, excellent interfacial bonding strength, and outstanding corrosion resistance are the key performance requirements that hot-dip galvanized high-strength fasteners must meet. The continuous improvement of these properties will not only significantly improve the overall performance of the fasteners themselves, but also expand their application range, enhance the safety, reliability, and service life of downstream products, and provide important support for the accelerated development of new energy, new infrastructure, and other fields. Therefore, focusing on these performance requirements, continuous innovation in the materials and processes of hot-dip galvanized high-strength fasteners is of great significance for promoting technological advancement in the industry and assisting in the construction of major national projects.

[0006] However, current hot-dip galvanized steel has shortcomings in terms of interfacial bonding strength, fastener strength, and corrosion resistance. First, regarding interfacial bonding strength, hot-dip galvanized fasteners produced using conventional processes often suffer from suboptimal bonding between the coating and the substrate. This is primarily due to inadequate pre-treatment of the fasteners prior to hot-dip galvanizing, resulting in the presence of oxides and impurities on the substrate surface, which impair effective wetting and metallurgical bonding between the zinc solution and the steel substrate. Furthermore, the brittle, hard, and massive zeta phase generated during the galvanizing process also weakens the interfacial bonding strength. Insufficient bonding strength can easily lead to flaking and cracking of the coating during use, resulting in a loss of protective properties and accelerated corrosion failure of the fastener. Second, regarding fastener strength, both current mainstream production processes have limitations. While using non-quenched and tempered steel can achieve higher strength through cold hardening, the complex alloy composition and high smelting costs result in expensive raw materials, and the high processing hardness contributes to high production costs. While traditional quenched and tempered steel production processes offer relatively low raw material costs, the energy consumption associated with quenching and high-temperature tempering is substantial, with electricity consumption approaching 600 kW h per ton of product, and production costs are also relatively high. Furthermore, the quenched martensitic structure is hard but has poor toughness. If tempering is not timely, it can easily lead to deformation and cracking, compromising fastener performance. Furthermore, in terms of corrosion resistance, while hot-dip galvanizing can significantly improve the corrosion resistance of steel fasteners, the corrosion resistance of the galvanized coating remains insufficient in some harsh environments, such as those with high salt spray and humidity, such as marine atmospheres and tidal splash zones. Long-term exposure to hot, humid, and chlorine-containing environments can easily lead to "white rust" on the coating, causing the formation of large quantities of zinc oxides and hydroxides, rapidly degrading the coating's protective properties. Furthermore, in some industrial atmospheres, the erosion of acid rain and sulfur-containing pollutants can accelerate the dissolution and destruction of the coating. This inadequate corrosion resistance limits the application range and lifespan of hot-dip galvanized fasteners.

[0007] In response to the above-mentioned shortcomings, it is urgent to develop a new hot-dip galvanized steel process. By optimizing the material composition of fasteners, improving the heat treatment system, and innovating the surface treatment process, while reducing production costs, the interface bonding strength between the coating and the substrate, the toughness of the fasteners, and the corrosion resistance of the coating can be improved from a mechanistic perspective to meet increasingly stringent application requirements. Summary of the Invention

[0008] (1) Technical problems solved The purpose of the present invention is to provide a high-strength hot-dip galvanized steel, a preparation method and its application in manufacturing fasteners, so as to solve the current problems of insufficient interface bonding strength, toughness of fasteners and corrosion resistance of the coating of hot-dip galvanized steel.

[0009] (2) Technical solution In order to achieve the above object, the present invention provides the following technical solutions: A method for preparing high-strength hot-dip galvanized steel comprises the following steps: S1: Cleaning carbon steel parts; S2: performing a stepwise heating of the carbon steel part obtained in step S1, and then performing a quenching treatment to obtain a quenched carbon steel part; S3: pickling and water washing the quenched carbon steel workpiece obtained in step S2, and performing a flux treatment using a flux solution; S4: Immersing the carbon steel part obtained in step S3 into a molten zinc solution for hot-dip galvanizing, and then sequentially performing centrifugal dezincification, water cooling, and discharging treatment to obtain the high-strength hot-dip galvanized steel.

[0010] Preferably, the composition of the carbon steel part is: C: 0.20-0.27%, B: 0.001-0.003%; Si: 0.02-0.06%, P: ≦0.020%, Cr: 0.10-0.20%, and the rest is Fe.

[0011] The carbon steel parts of this invention are low-carbon boron steel, a compositional design that significantly improves the steel's strength and toughness. An appropriate carbon content ensures the steel's strength, while the addition of trace amounts of boron refines the grain size, enhancing the steel's plasticity and toughness. Furthermore, the addition of silicon and chromium improves the steel's hardenability and wear resistance, further enhancing the overall mechanical properties of hot-dip galvanized steel.

[0012] Preferably, in step S2, the carbon steel part obtained in step S1 is subjected to stepwise heating to slightly decarburize the surface of the carbon steel part; The process parameters for the step-temperature ramp are as follows: first, the temperature is increased from room temperature to 340-350°C at a rate of 1-5°C / min, then to 550-560°C at a rate of 1-3°C / min, and then to the quenching temperature at a rate of 0.5-1.5°C / min. The quenching temperature is 720-850°C. The heating atmosphere for the step-temperature ramp is a mixture of nitrogen and methanol with a carbon potential of 0.08%-0.12%. The methanol gas is generated by directly dripping liquid methanol into the heating area.

[0013] Preferably, in step S2, the quenching liquid used during the quenching is a 2% by mass polyethylene glycol aqueous solution, and the temperature of the quenching liquid is 35-40°C; The hardness of the quenched carbon steel part is greater than 40HRC, and the thickness of the surface micro-decarburization layer is 0.03-0.08mm.

[0014] Step S2 of the present invention cleverly balances the strength, hardness, and corrosion resistance of carbon steel parts through a quenching process. A stepwise heating process is employed, precisely controlling the heating rate and the carbon potential of the protective atmosphere to form a micro-decarburized layer on the carbon steel surface. While this low-carbon layer slightly reduces surface hardness, it significantly improves the toughness and crack resistance of the part, while also enhancing corrosion resistance after hot-dip galvanizing. This innovative method provides an effective approach for achieving high-performance hot-dip galvanized steel parts, successfully balancing the two key performance indicators of strength and corrosion resistance. The quenching treatment of the present invention cleverly combines the advantages of the micro-decarburized layer and martensitic structure to achieve an optimal balance of properties. The micro-decarburized layer alleviates stress concentration during the hot-dip galvanizing process, improving the coating quality and corrosion resistance. The quenching treatment forms a high-strength, high-hardness martensitic structure, achieving a hardness exceeding 40 HRC and significantly enhancing load-bearing capacity. The choice of quenching liquid (2% polyalkylene glycol aqueous solution) and optimized process parameters (35-40°C) ensure a uniform martensitic structure and consistent hardness distribution. The thickness of the micro-decarburization layer is precisely controlled at 0.03~0.08mm, which provides appropriate toughness and crack resistance while ensuring surface hardness, effectively balancing strength and corrosion resistance.

[0015] Preferably, in step S3, the quenched carbon steel part obtained in step S2 is sequentially subjected to pickling, water washing, and flux plating treatment within 1 hour after discharge; The pickling is performed using a pickling agent, and the pickling time is 4 to 6 minutes. The preparation method of the pickling agent comprises the following steps: adding ferrous chloride to hydrochloric acid with a mass fraction of 5 to 6%, stirring and mixing to obtain the pickling agent; the concentration of ferrous chloride in the pickling agent is 50 to 100 g / L; The flux-plating solution is an aqueous solution containing 200-250 g / L ammonium chloride and 5-10 g / L zinc chloride, and the pH value of the flux-plating solution is adjusted to 4-5 with hydrochloric acid. That is, the preparation method of the flux-plating solution comprises the following steps: adding ammonium chloride and zinc chloride to water, stirring and mixing, and adjusting the pH value of the solution to 4-5 with hydrochloric acid to obtain the flux-plating solution, wherein the content of ammonium chloride in the flux-plating solution is 200-250 g / L, and the content of zinc chloride in the flux-plating solution is 5-10 g / L; The temperature of the plating assist treatment is 30-40° C., and the time is 30-90 seconds.

[0016] Step S3 of the present invention optimizes the pre-treatment process of hot-dip galvanized carbon steel parts, including three key steps: pickling, water washing and flux plating, aiming to obtain high-quality zinc coating, improve corrosion resistance and ensure overall strength. Pickling uses hydrochloric acid solution and ferrous chloride accelerator to remove surface oxide layer and impurities, creating good conditions for zinc plating. Water washing removes residual acid and impurities to prevent contamination of flux plating solution. Fluid plating treatment uses ammonium chloride and zinc chloride to form a zinc-affinity chloride layer, which improves the wettability and bonding strength of zinc solution to steel base. By carefully controlling various process parameters such as pickling efficiency, flux plating solution concentration, pH value, temperature and time, high bonding strength, density and uniformity of the zinc coating are achieved. This optimized design significantly improves corrosion resistance while ensuring the strength of the parts, which is of great significance to obtaining hot-dip galvanized carbon steel parts with excellent comprehensive performance.

[0017] Preferably, in step S4, the composition of the molten zinc solution is: Fe: 0.2-0.35%, Ni: 0.030-0.045%, Al: 0.015-0.025%, and the rest is Zn; The temperature of the hot-dip galvanizing is 520-540° C., and the time is 25-35 seconds.

[0018] Preferably, in step S5, the rotation speed of the centrifugal dezincification is 550-650 rpm; and the water cooling temperature is 60-80°C.

[0019] Step S4 of the present invention optimizes the hot-dip galvanizing process, aiming to obtain a galvanized layer with excellent performance and improve the coating strength, interface bonding and corrosion resistance. By optimizing the composition of the molten zinc solution (adding Fe, Ni, and Al elements), controlling the galvanizing process parameters (galvanizing temperature of 520~540℃, galvanizing time of 25~35s), and adopting centrifugal dezincification and water cooling and other coordinated regulation, the optimization of structure and performance is achieved. The Fe element improves hardness and wear resistance, the Ni element refines the structure and improves toughness, and the Al element forms a barrier layer to improve interface bonding. Centrifugal dezincification ensures uniform surface quality and thickness, and water cooling inhibits the formation of brittle phases and improves toughness. The combined effect of these optimization measures significantly improves the strength characteristics, interface bonding performance and corrosion resistance of the galvanized layer, providing important guidance for obtaining high-performance hot-dip galvanized carbon steel parts.

[0020] In general, the innovative method for preparing high-strength hot-dip galvanized steel of the present invention is based on improved low-carbon boron steel. By optimizing the heat treatment process, it cleverly utilizes the heat of the hot-dip galvanizing process to achieve the tempering effect and the formation of the galvanized layer. This process innovation of "using zinc instead of fire" eliminates the traditional separate tempering process, effectively solving the problems of easy cracking due to quenching without tempering, and abnormal growth of the galvanized layer caused by quenched martensite. At the same time, this method greatly simplifies the preparation process, saving 110 to 130 degrees of electricity per ton of fasteners, and controlling the consumption of new water within 200 kg, reflecting significant energy-saving, cost-reduction and environmental protection benefits. This process innovation stems from a deep understanding and clever combination of the quenching and tempering mechanism and the hot-dip galvanizing mechanism. It not only ensures the high strength and coating quality of the product, but also provides a new idea for the green and efficient preparation of hot-dip galvanized steel, which has important implications for promoting the high-quality development of the manufacturing industry.

[0021] The present invention also discloses a high-strength hot-dip galvanized steel, which is prepared by the above-mentioned preparation method; The high-strength hot-dip galvanized steel includes a carbon steel layer, a transition layer and a galvanized layer located on the carbon steel layer. The transition layer is located between the carbon steel layer and the galvanized layer. The thickness of the transition layer is 20-60 μm, and the thickness of the galvanized layer is 40-80 μm.

[0022] In this hot-dip galvanized steel solution, the transition layer thickness is controlled between 20 and 60 μm, the carbon steel layer is made of low-carbon boron steel, and the zinc coating thickness is 40 to 80 μm. These design considerations significantly impact the interfacial bonding strength, the toughness and toughness of the fastener, and the corrosion resistance of the coating. First, a transition layer thickness within the 20-60 μm range ensures good bonding strength while avoiding the brittleness associated with excessive thickness. A moderate transition layer thickness promotes a stable, continuous interface, providing sufficient bonding area while minimizing the effects of thermal and residual stresses, reducing the risk of interfacial cracking. Second, a zinc coating thickness of 40 to 80 μm provides adequate corrosion protection, extending the service life of the fastener. A thicker zinc coating acts as a sacrificial anode, corroding preferentially and thus protecting the underlying steel substrate. Furthermore, a thicker zinc coating provides a longer corrosion pathway, slowing the penetration of corrosive media into the steel substrate. Importantly, the zinc coating thickness should be kept within a reasonable range, as this can compromise the assembly precision and appearance of the fastener. In summary, this hot-dip galvanized steel solution achieves a balance between interfacial bonding strength, fastener toughness, and coating corrosion resistance through the rational design of the transition layer thickness, the selection of low-carbon boron steel as the carbon steel layer, and controlled galvanized layer thickness, meeting the application requirements of high-performance fasteners. The optimized transition layer thickness ensures interface stability, the use of low-carbon boron steel enhances fastener strength and toughness, and the appropriate galvanized layer thickness provides reliable corrosion protection. This comprehensive performance improvement lays the foundation for the application of hot-dip galvanized steel in the high-end fastener market.

[0023] Preferably, the transition layer contains ζ-FeZn 13 ,δ-FeZn 10 and Fe2B.

[0024] The strong metallurgical bonding between the transition layer and the carbon steel layer is the basis for ensuring the overall performance of hot-dip galvanized steel. The presence and composition of the transition layer also help to improve the strength of galvanized steel. 13 and δ-FeZn 10 It is a Fe-Zn intermetallic compound, and its hardness and strength are higher than that of pure zinc coating. The presence of these hard phases in the transition layer improves the bearing capacity of the coating. At the same time, the hard Fe2B particles are dispersed in the ζ-FeZn 13 and δ-FeZn 10 In the matrix, Fe2B acts as a second phase reinforcement, similar to hard particle-reinforced composites. The Fe2B particles hinder dislocation motion, increasing the yield strength and plastic deformation resistance of the transition layer. The overall high strength of the transition layer is then transferred to the carbon steel matrix through metallurgical bonding, ultimately improving the strength of hot-dip galvanized steel.

[0025] In addition, the ζ-FeZn in the transition layer 13and δ-FeZn 10 Although they have high hardness, they still maintain good electrochemical activity and can form effective sacrificial anode protection with the pure zinc coating on the surface. The potential difference between the transition layer and the surface zinc coating causes corrosion to occur preferentially in the surface layer, thus protecting the carbon steel matrix. Fe2B exists in the transition layer in the form of inert particles. It does not participate in the electrochemical reaction, but can fill the ζ-FeZn 13 and δ-FeZn 10 The transition layer forms a three-layer protective structure of "galvanized layer-transition layer-carbon steel layer", which greatly improves the corrosion resistance life of hot-dip galvanized steel.

[0026] In summary, the hot-dip galvanized steel of the present invention introduces a layer containing ζ-FeZn between the galvanized layer and the carbon steel layer. 13 ,δ-FeZn 10 and Fe2B transition layer. ζ-FeZn 13 ,δ-FeZn 10 The presence of Fe2B and its composite strengthening effect give the transition layer and the entire galvanized steel high strength properties. In addition, the transition layer, the surface galvanized layer and the carbon steel matrix form a three-layer protection, ζ-FeZn 13 and δ-FeZn 10 The sacrificial anode provides protection, while Fe2B blocks corrosion pathways, collectively enhancing the corrosion resistance of hot-dip galvanized steel. This invention, through optimized design of the transition layer composition and structure, creates a "bridge" between the galvanized layer and the carbon steel substrate that combines high bonding strength, high strength, and high corrosion resistance, ultimately resulting in a new type of hot-dip galvanized steel with excellent overall performance.

[0027] Preferably, the transition layer contains ζ-FeZn 13 Form a lattice matching interface with Fe2B.

[0028] The ζ-FeZn in the transition layer of the present invention 13 It forms a lattice matching interface with Fe2B. This special interface structure is conducive to significantly improving the metallurgical bonding between the coating and the steel base. The lattice matching interface refers to the interface between the two phases with consistent lattice orientation and good structural matching. This interface has high bonding strength and can effectively inhibit interface cracking and coating peeling. 13 The formation of a lattice matching interface with Fe2B means that the atomic arrangement at the interface is more coordinated and the interface bonding is tighter. Compared with the general non-lattice matching interface, the lattice matching interface greatly reduces the interface energy and reduces the interface defects, thus obtaining an extraordinary interface bonding performance. 13 It forms a lattice matching interface with Fe2B, significantly improving the interface bonding strength and effectively solving the problem of coating peeling.

[0029] Preferably, the Fe2B columnar crystals in the transition layer present a tooth-like structure and are perpendicular to the transition layer interface; the average spacing of the Fe2B columnar crystals is 2-4 μm; The ζ-FeZn in the transition layer 13 and δ-FeZn 10 Evenly distributed among the Fe2B columnar crystals.

[0030] In the present invention, the Fe2B columnar crystals in the transition layer present a tooth-like structure, which is perpendicular to the transition layer interface and has an average spacing of 2 to 4 μm. 13 ,δ-FeZn 10 Uniformly distributed between the Fe2B columnar crystals. This structure can improve the material performance through the following mechanisms: First, the Fe2B columnar crystals grow perpendicular to the transition layer interface to form a tooth-like structure, which can significantly increase the mechanical locking effect between the galvanized layer and the steel substrate and improve the interface bonding strength. The tooth-like structure increases the interface area and provides more bonding sites. At the same time, the vertically grown columnar crystals can effectively resist shear stress and prevent interface shedding. Secondly, the ζ-FeZn13 and δ-FeZn 10 Evenly distributed between Fe2B columnar crystals, forming a composite structure. These intermetallic compounds have high hardness and strength, which can enhance the mechanical properties of the transition layer. At the same time, the composite structure formed by them and Fe2B columnar crystals can effectively hinder crack propagation and improve the strength and toughness of fasteners. In addition, Fe2B, ζ-FeZn 13 ,δ-FeZn 10 The presence of compounds such as ζ-FeZn in the transition layer can improve the corrosion resistance of the transition layer and delay the penetration of the corrosive medium into the steel matrix. Finally, by controlling the average spacing of Fe2B columnar crystals within the range of 2~4μm, it is possible to avoid the brittleness problem caused by over-dense columnar crystals while ensuring good interface bonding and mechanical properties. 13 ,δ-FeZn 10 Evenly distributed between Fe2B columnar crystals, it can comprehensively improve the interface bonding strength of hot-dip galvanized steel, the toughness of fasteners, and the corrosion resistance of the coating by increasing the density of the transition layer, forming a composite structure, hindering crack propagation, reducing stress concentration, and improving corrosion resistance. This design takes advantage of the advantages of different phases and achieves good comprehensive performance through uniform distribution and compounding. Of course, in actual applications, it is also necessary to control the content and distribution of each phase through process optimization and composition regulation to obtain the best performance combination.

[0031] Preferably, the α-Fe in the carbon steel layer and the Fe2B phase in the transition layer form a lattice matching interface.

[0032] In this hot-dip galvanized steel solution, the α-Fe phase in the carbon steel layer forms a lattice-matched interface with the Fe2B phase in the transition layer. This unique interface structure significantly impacts the material's interfacial bonding strength, the fastener's toughness, and the coating's corrosion resistance. A lattice-matched interface refers to a continuous lattice arrangement between the two phases, matching lattice parameters, and a close, continuous atomic arrangement at the interface, without significant interface deviations or defects. The lattice-matched interface between the α-Fe and Fe2B phases signifies good structural matching and chemical compatibility, resulting in a low energy state and high stability at the interface. This lattice-matched interface significantly enhances interfacial bonding strength, reduces stress concentration, and inhibits the initiation and propagation of microcracks. The close, continuous atomic arrangement facilitates smooth load transfer at the interface, reducing the risk of interfacial slip and debonding. Furthermore, the lattice-matched interface reduces residual and thermal stresses at the interface, improving its thermal stability and minimizing interfacial damage caused by temperature fluctuations during use. Furthermore, the lattice-matched interface between the α-Fe and Fe2B phases also enhances the fastener's toughness. Fe2B is a ceramic phase with high hardness and strength, while α-Fe exhibits excellent plasticity and toughness. The lattice-matched interface between the two phases means that their mechanical properties are well matched, achieving an effective combination of hardness and toughness. The Fe2B phase hinders dislocation motion, increasing the material's strength, while the α-Fe phase absorbs energy through plastic deformation, improving the material's toughness. The lattice-matched interface between the two phases ensures uniform load transfer, avoids stress concentration, and reduces crack initiation and propagation at the interface, thereby improving the fastener's fracture toughness and fatigue performance. Finally, the lattice-matched interface between the α-Fe and Fe2B phases also positively impacts the corrosion resistance of the coating. A lattice-matched interface means that the atoms at the interface are tightly packed, without significant defects or gaps, effectively preventing the penetration and diffusion of corrosive media at the interface. This compact interface structure reduces corrosion pathways and delays the onset and progression of corrosion. Furthermore, the Fe2B phase itself possesses high chemical stability and corrosion resistance, acting as a barrier layer to prevent the penetration of corrosive media into the steel substrate, further enhancing the corrosion resistance of the coating. In summary, in this hot-dip galvanized steel solution, the α-Fe in the carbon steel layer forms a lattice-matched interface with the Fe2B phase in the transition layer. This optimizes the overall material performance by increasing interfacial bonding strength, improving the strength and toughness of the fastener, and enhancing the corrosion resistance of the coating. The presence of the lattice-matched interface ensures interface stability and continuity, promotes uniform load transfer and stress distribution, and hinders the penetration of corrosive media, providing important support for the development of high-performance hot-dip galvanized steel fasteners.

[0033] The present invention also provides an application of high-strength hot-dip galvanized steel, which is applied to grade 8 to grade 10 nut hot-dip galvanized layer fasteners.

[0034] Beneficial effects:

[0035] 1. This method for producing high-strength hot-dip galvanized steel achieves a balance between interfacial bonding strength, fastener toughness, and corrosion resistance by optimizing the transition layer thickness (20-60 μm), selecting low-carbon boron steel as the substrate, and controlling the galvanized layer thickness (40-80 μm). The production process includes a step-by-step temperature ramp to form a micro-decarburized layer (0.03-0.08 mm), quenching, a carefully controlled pretreatment process, hot-dip galvanizing (520-540°C, 25-35 seconds) with the addition of Fe, Ni, and Al elements, centrifugal dezincification, and water cooling. The innovative use of the galvanizing temperature instead of a separate tempering step simplifies the process, saving 110-130 degrees Celsius per ton of fasteners and keeping fresh water consumption to less than 200 kg. This method addresses challenges inherent in conventional processes, significantly improving the overall performance of the finished product while simultaneously achieving energy savings, cost reduction, and environmental benefits. It provides a new approach for the green and efficient production of hot-dip galvanized steel.

[0036] 2. The hot-dip galvanized steel of the present invention introduces ζ-FeZn between the galvanized layer and the carbon steel layer. 13 ,δ-FeZn 10 and Fe2B transition layer, and through ζ-FeZn 13 It forms a lattice matching interface with Fe2B to improve the interface bonding strength and solve the problem of coating peeling; at the same time, it uses the composite strengthening effect of the three compounds to improve the overall strength; and forms a three-layer protective structure, in which ζ-FeZn13 and δ-FeZn 10 The sacrificial anode provides protection, while Fe2B blocks corrosion channels, enhancing corrosion resistance. This invention creates a "bridge" between the galvanized layer and the carbon steel substrate that combines high bonding strength, high strength, and high corrosion resistance, ultimately yielding a new type of hot-dip galvanized steel with excellent overall performance.

[0037] 3. The transition layer of the present invention comprises Fe2B tooth-shaped columnar crystals with an average spacing of 2~4μm and ζ-FeZn uniformly distributed therebetween. 13 and δ-FeZn 10 The composite structure can increase the bonding strength by increasing the interface bonding area, while enhancing the mechanical properties of the transition layer, hindering crack propagation, and improving the strength and toughness of the fastener. The presence of intermetallic compounds also improves corrosion resistance and delays the penetration of corrosive media. Reasonable control of the average spacing of Fe2B columnar crystals not only ensures good interface bonding and mechanical properties, but also avoids the brittleness problem caused by overcrowding. The present invention comprehensively improves the interface bonding strength of hot-dip galvanized steel, the strength and toughness of the fastener, and the corrosion resistance of the coating.

[0038] 4. In the present invention, the α-Fe in the carbon steel layer and the Fe2B in the transition layer form a coherent interface lattice match, achieving a defect-free interface with continuous lattice arrangement and dense atomic arrangement. This structure significantly improves the interface bonding strength, reduces stress concentration, inhibits the initiation of microcracks, reduces interface residual stress and thermal stress, and improves the thermal stability of the interface. At the same time, the combination of α-Fe and Fe2B achieves an effective combination of hardness and toughness, improving the fracture toughness and fatigue performance of the fastener. In addition, the tight coherent interface structure and the high corrosion resistance of Fe2B jointly prevent the penetration and diffusion of corrosive media, thereby improving the corrosion resistance of the coating. The present invention achieves comprehensive optimization of material properties from multiple aspects, including interface bonding, mechanical properties, and corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is the XRD phase analysis of the hot-dip galvanized steel prepared in Example 1 of the present invention.

[0040] Figure 2 This is a transmission electron microscope photograph of the interface between α-Fe and Fe2B in the hot-dip galvanized steel prepared in Example 1 of the present invention.

[0041] Figure 3 Fe2B and ζ-FeZn in the hot-dip galvanized steel prepared in Example 1 of the present invention 13 Transmission electron microscopy photograph of the interface.

[0042] Figure 4 This is the microstructural morphology of the hot-dip galvanized steel prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0043] To make the purpose, technical solutions and advantages of the embodiments of the present invention more clear, the technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings in the embodiments of the present invention.

[0044] Example 1:

[0045] A method for preparing high-strength hot-dip galvanized steel comprises the following steps: S1: Low carbon boron steel is reformed and formed into carbon steel parts; the composition of low carbon boron steel is: C: 0.20%, B: 0.001%; ​​Si: 0.02%, P: ≤ 0.020%, Cr: 0.10%, and the rest is Fe.

[0046] S2: Use 5% by mass hydrochloric acid to pickle and remove rust on the surface of the carbon steel parts. Then use a 50% by mass acetone and water mixture to remove stains on the surface of the carbon steel parts, and then dry.

[0047] S3: The carbon steel part cleaned in step S2 is subjected to a stepwise heating process to achieve micro-decarburization of the carbon steel part's surface. After the stepwise heating process is completed, the part is immediately quenched and inspected. Only qualified carbon steel parts are obtained. The stepwise heating process parameters are: from room temperature to 340°C at a rate of 1°C / min, then to 550°C at a rate of 1°C / min, and then to the quenching temperature at a rate of 0.5°C / min. The quenching temperature is 720°C. The heating atmosphere for the stepwise heating process is a mixture of nitrogen and methanol with a carbon potential of 0.08%. The quenching liquid used is a 2% by mass aqueous solution of polyalkylene glycol at a temperature of 35°C. The hardness of the quenched carbon steel part is greater than 40 HRC, and the thickness of the micro-decarburization layer on the surface is 0.03 mm.

[0048] S4: The quenched carbon steel part obtained in step S3 is pickled and washed with water within 1 hour after being discharged, and a flux treatment is performed using a flux solution; The pickling is carried out using a pickling agent for 4 minutes. The preparation method of the pickling agent comprises the following steps: adding ferrous chloride to 5% hydrochloric acid by mass, stirring and mixing to obtain the pickling agent; the concentration of ferrous chloride in the pickling agent is 50 g / L; The flux solution is an aqueous solution containing 200 g / L ammonium chloride and 5 g / L zinc chloride. The pH value of the flux solution is adjusted to 4 with hydrochloric acid. The flux treatment temperature is 30°C and the time is 30s.

[0049] S5: Immerse the carbon steel part obtained in step S4 in a molten zinc solution for hot-dip galvanizing, and then perform centrifugal dezincification, water cooling, and discharging treatment in sequence to obtain high-strength hot-dip galvanized steel.

[0050] The composition of the molten zinc solution is: Fe: 0.2%, Ni: 0.030%, Al: 0.015%, and the remainder is Zn. The hot-dip galvanizing temperature is 520°C, and the hot-dip galvanizing time is 25 seconds. The centrifugal dezincification speed is 550 rpm, and the water cooling temperature is 60°C.

[0051] The high-strength hot-dip galvanized steel of this embodiment includes a carbon steel layer, a transition layer and a galvanized layer located on the carbon steel layer. The transition layer is located between the carbon steel layer and the galvanized layer. The thickness of the galvanized layer is 40 μm, and the thickness of the transition layer is 20 μm. The transition layer contains ζ-FeZn 13 ,δ-FeZn 10 and Fe2B;ζ-FeZn in the transition layer 13 It forms a lattice matching interface with Fe2B; the Fe2B columnar crystals in the transition layer present a tooth-like structure and are perpendicular to the transition layer interface; the average spacing of the Fe2B columnar crystals is 2μm; the ζ-FeZn in the transition layer 13 and δ-FeZn10 Evenly distributed between the Fe2B columnar crystals; the α-Fe in the carbon steel layer and the Fe2B phase in the transition layer form a lattice matching interface.

[0052] The hot-dip galvanized steel prepared in Example 1 of the present invention was comprehensively characterized by various analytical methods. XRD phase analysis results ( Figure 1 ) clearly shows the multilayer structure of the material, confirming that the transition layer is composed of ζ-FeZn 13 ,δ-FeZn 10 The carbon steel layer is composed of a mixture of Fe2B and α-Fe and Fe3C phases, while the galvanized layer is mainly composed of η-Zn phase. Further microstructural analysis was achieved by transmission electron microscopy. Figure 2 and Figure 3 α-Fe and Fe2B and Fe2B and ζ-FeZn are shown respectively 13 The interfaces between them all show lattice matching characteristics, indicating that the interlayers are tightly bonded, which is beneficial to improving the overall performance of the material. Figure 4 ) revealed the layered structure of hot-dip galvanized steel, consisting, from the outside in, of a galvanized layer, a transition layer, and a carbon steel layer. Of particular note, the Fe2B phase in the transition layer exhibits a unique columnar crystal morphology. These crystals exhibit a serrated structure and grow perpendicular to the transition layer interface. This unique microstructure may positively impact the material's mechanical properties and corrosion resistance. In summary, these analytical results not only confirm that the hot-dip galvanized steel prepared in this invention possesses the desired multilayered structure and phase composition, but also reveal its unique micromorphological characteristics, providing important insights into material properties.

[0053] Example 2:

[0054] A method for preparing high-strength hot-dip galvanized steel comprises the following steps: S1: Low carbon boron steel is reformed and formed into carbon steel parts; the composition of low carbon boron steel is C: 0.22%, B: 0.0016%; Si: 0.03%, P: ≤ 0.020%, Cr: 0.13%, and the rest is Fe.

[0055] S2: Use 5% by mass hydrochloric acid to pickle and remove rust on the surface of the carbon steel parts. Then use a 50% by mass acetone and water mixture to remove stains on the surface of the carbon steel parts, and then dry.

[0056] S3: The carbon steel part cleaned in step S2 is subjected to a stepwise heating process to achieve micro-decarburization of the carbon steel part's surface. After the stepwise heating process is completed, the part is immediately quenched and inspected. Only qualified carbon steel parts are obtained. The stepwise heating process parameters are: from room temperature to 342°C at a rate of 2°C / min, then to 552°C at a rate of 1.5°C / min, and then to the quenching temperature at a rate of 0.8°C / min, with a quenching temperature of 759°C. The heating atmosphere for the stepwise heating process is a mixture of nitrogen and methanol with a carbon potential of 0.09%. The quenching liquid used is a 2% by mass aqueous solution of polyalkylene glycol at a temperature of 37°C. The hardness of the quenched carbon steel part is greater than 40 HRC, and the thickness of the micro-decarburization layer on the surface is 0.045 mm.

[0057] S4: The quenched carbon steel part obtained in step S3 is pickled and washed with water within 1 hour after being discharged, and a flux treatment is performed using a flux solution; The pickling is performed using a pickling agent for 5 minutes. The preparation method of the pickling agent comprises the following steps: adding ferrous chloride to 5.3% hydrochloric acid by mass, stirring and mixing to obtain the pickling agent; the concentration of ferrous chloride in the pickling agent is 65 g / L; The flux solution is an aqueous solution containing 215 g / L ammonium chloride and 7 g / L zinc chloride. The pH value of the flux solution is adjusted to 4.3 with hydrochloric acid. The flux treatment temperature is 33° C. and the time is 48 s.

[0058] S5: The carbon steel article obtained in step S4 is immersed in a molten zinc bath for hot-dip galvanizing. Centrifugal dezincification, water cooling, and discharging are then performed sequentially to obtain high-strength hot-dip galvanized steel. The composition of the molten zinc bath is: Fe: 0.25%, Ni: 0.035%, Al: 0.018%, and the remainder is Zn. The hot-dip galvanizing process parameters are: hot-dip galvanizing temperature: 526°C, hot-dip galvanizing time: 28 seconds, centrifugal dezincification speed: 580 rpm, and water cooling temperature: 66°C.

[0059] The high-strength hot-dip galvanized steel of this embodiment includes a carbon steel layer, a transition layer and a galvanized layer located on the carbon steel layer. The transition layer is located between the carbon steel layer and the galvanized layer. The thickness of the galvanized layer is 52 μm. The thickness of the transition layer is 32 μm. The transition layer contains ζ-FeZn 13 ,δ-FeZn 10 and Fe2B;ζ-FeZn in the transition layer 13 The Fe2B columnar crystals in the transition layer have a dentate structure and are perpendicular to the transition layer interface. The average spacing of the Fe2B columnar crystals is 2.3 μm. The ζ-FeZn in the transition layer 13 and δ-FeZn 10Evenly distributed between the Fe2B columnar crystals; the α-Fe in the carbon steel layer and the Fe2B phase in the transition layer form a lattice matching interface.

[0060] Example 3:

[0061] A method for preparing high-strength hot-dip galvanized steel comprises the following steps: S1: Low carbon boron steel is reformed and formed into carbon steel parts; the composition of low carbon boron steel is C: 0.24%, B: 0.0022%; Si: 0.04%, P: ≤ 0.020%, Cr: 0.16%, and the rest is Fe.

[0062] S2: Use 5% by mass hydrochloric acid to pickle and remove rust on the surface of the carbon steel parts. Then use a 50% by mass acetone and water mixture to remove stains on the surface of the carbon steel parts, and then dry.

[0063] S3: The carbon steel part cleaned in step S2 is subjected to a stepwise heating process to achieve micro-decarburization of the carbon steel part's surface. After the stepwise heating process is completed, the part is immediately quenched and inspected. Only qualified carbon steel parts are obtained. The stepwise heating process parameters are: from room temperature to 356°C at a rate of 3°C / min, then to 555°C at a rate of 2°C / min, and then to the quenching temperature at a rate of 1°C / min. The quenching temperature is 798°C. The heating atmosphere for the stepwise heating process is a mixture of nitrogen and methanol with a carbon potential of 0.10%. The quenching liquid used is a 2% (mass fraction) aqueous solution of polyalkylene glycol at a temperature of 38°C. The hardness of the quenched carbon steel part is greater than 40 HRC, and the thickness of the micro-decarburization layer on the surface is 0.06 mm.

[0064] S4: The quenched carbon steel parts obtained in S3 are pickled and washed with water within 1 hour after being discharged, and a flux treatment is performed using a flux solution; The pickling is performed using a pickling agent for 5 minutes. The preparation method of the pickling agent comprises the following steps: adding ferrous chloride to 5.6% hydrochloric acid, stirring and mixing to obtain the pickling agent; the concentration of ferrous chloride in the pickling agent is 80 g / L; The flux solution is an aqueous solution containing 230 g / L ammonium chloride and 8 g / L zinc chloride. The pH value of the flux solution is adjusted to 4.6 with hydrochloric acid. The flux treatment temperature is 36°C and the time is 66 seconds.

[0065] S5: The carbon steel parts obtained in S4 are immersed in molten zinc for hot-dip galvanizing. Centrifugal dezincification, water cooling, and discharge are then performed sequentially to obtain high-strength hot-dip galvanized steel. The composition of the molten zinc solution is: Fe: 0.29%, Ni: 0.039%, Al: 0.021%, and the remainder is Zn. The hot-dip galvanizing process parameters are: hot-dip galvanizing temperature: 532°C, hot-dip galvanizing time: 31 seconds, centrifugal dezincification speed: 610 rpm, and water cooling temperature: 72°C.

[0066] The high-strength hot-dip galvanized steel of this embodiment includes a carbon steel layer, a transition layer and a galvanized layer located on the carbon steel layer. The transition layer is located between the carbon steel layer and the galvanized layer. The thickness of the galvanized layer is 64 μm. The thickness of the transition layer is 44 μm. The transition layer contains ζ-FeZn 13 ,δ-FeZn 10 and Fe2B;ζ-FeZn in the transition layer 13 It forms a lattice matching interface with Fe2B; the Fe2B columnar crystals in the transition layer present a tooth-like structure and are perpendicular to the transition layer interface; the average spacing of the Fe2BB columnar crystals is 3μm; the ζ-FeZn in the transition layer 13 and δ-FeZn 10 Evenly distributed between the Fe2B columnar crystals; the α-Fe in the carbon steel layer and the Fe2B phase in the transition layer form a lattice matching interface.

[0067] Example 4:

[0068] A method for preparing high-strength hot-dip galvanized steel comprises the following steps: S1: Low carbon boron steel is reformed and formed into carbon steel parts; the composition of low carbon boron steel is C: 0.27%, B: 0.003%; Si: 0.06%, P: ≤ 0.020%, Cr: 0.20%, and the rest is Fe.

[0069] S2: Use 5% by mass hydrochloric acid to pickle and remove rust on the surface of the carbon steel parts. Then use a 50% by mass acetone and water mixture to remove stains on the surface of the carbon steel parts, and then dry.

[0070] S3: The carbon steel part cleaned in step S2 is subjected to a stepwise heating process to achieve micro-decarburization of the carbon steel part's surface. After the stepwise heating process is completed, the part is immediately quenched and inspected. Only qualified carbon steel parts are obtained. The stepwise heating process parameters are: from room temperature to 350°C at a rate of 5°C / min, then to 560°C at a rate of 3°C / min, and then to the quenching temperature at a rate of 1.5°C / min. The quenching temperature is 850°C. The heating atmosphere for the stepwise heating process is a mixture of nitrogen and methanol with a carbon potential of 0.12%. The quenching liquid used is a 2% by mass aqueous solution of polyalkylene glycol at a temperature of 40°C. The hardness of the quenched carbon steel part is greater than 40 HRC, and the thickness of the micro-decarburization layer on the surface is 0.08 mm.

[0071] S4: The quenched carbon steel part obtained in step S3 is pickled and washed with water within 1 hour after being discharged, and a flux treatment is performed using a flux solution; The pickling is performed using a pickling agent for 6 minutes. The preparation method of the pickling agent comprises the following steps: adding ferrous chloride to 6% hydrochloric acid by mass, stirring and mixing to obtain the pickling agent; the concentration of ferrous chloride in the pickling agent is 100 g / L; The flux solution is an aqueous solution containing 250 g / L ammonium chloride and 10 g / L zinc chloride. The pH value of the flux solution is adjusted to 5 with hydrochloric acid. The temperature of the flux treatment is 30~40℃, and the time is 30~90s.

[0072] S5: The carbon steel article obtained in step S4 is immersed in a molten zinc bath for hot-dip galvanizing. Centrifugal dezincification, water cooling, and discharging are then performed sequentially to obtain high-strength hot-dip galvanized steel. The composition of the molten zinc bath is: Fe: 0.35%, Ni: 0.045%, Al: 0.025%, and the remainder is Zn. The hot-dip galvanizing process parameters are: hot-dip galvanizing temperature: 540°C, hot-dip galvanizing time: 35 seconds, centrifugal dezincification speed: 650 rpm, and water cooling temperature: 80°C.

[0073] The high-strength hot-dip galvanized steel of this embodiment includes a carbon steel layer, a transition layer and a galvanized layer located on the carbon steel layer. The transition layer is located between the carbon steel layer and the galvanized layer. The thickness of the galvanized layer is 80 μm, and the thickness of the transition layer is 60 μm. The transition layer contains ζ-FeZn 13 ,δ-FeZn 10 and Fe2B;ζ-FeZn in the transition layer 13 It forms a lattice matching interface with Fe2B; the Fe2B columnar crystals in the transition layer present a tooth-like structure and are perpendicular to the transition layer interface; the average spacing of the Fe2B columnar crystals is 4μm; the ζ-FeZn in the transition layer 13 and δ-FeZn 10Evenly distributed between the Fe2B columnar crystals; the α-Fe in the carbon steel layer and the Fe2B phase in the transition layer form a lattice matching interface.

[0074] Comparative Example 1: The process is essentially the same as Example 1, except that the quenching temperature in the step-by-step temperature increase in step S3 is 900°C, while the other parameters remain unchanged. Therefore, a higher quenching temperature accelerates the diffusion of carbon atoms and promotes surface decarburization. The final carbon steel part has a hardness of 38 HRC and a decarburized layer thickness of 0.1 mm.

[0075] Comparative Example 2: The process is essentially the same as Example 1, except that the carbon potential of the heating atmosphere during the stepwise heating in step S3 is set to 0.06%, while all other parameters remain unchanged. A lower carbon potential increases the carbon concentration gradient between the steel surface and the surrounding atmosphere, promoting outward diffusion of carbon atoms and surface decarburization. The final carbon steel part has a hardness of 36 HRC and a decarburized layer thickness of 0.11 mm.

[0076] Comparative Example 3: The method is basically the same as Example 1, except that the hot-dip galvanizing temperature in step S5 is 480° C. A lower temperature will reduce the diffusion reaction between Fe and Zn, thereby reducing the thickness of the transition layer. Therefore, the thickness of the transition layer in this embodiment is 15 μm.

[0077] Comparative Example 4: The method is basically the same as Example 1, except that the hot-dip galvanizing temperature in step S5 is 580° C. A higher temperature will accelerate the diffusion reaction between Fe and Zn, thereby increasing the thickness of the transition layer. Therefore, the thickness of the transition layer in this embodiment is 83 μm.

[0078] Performance testing: Appearance Inspection: The appearance quality testing of hot-dip galvanized steel complies with the GB / T13912-2002 "Hot-Dip Galvanizing Standard," primarily evaluating the surface characteristics of the coating. Inspection includes surface smoothness, defect detection (such as nodules, roughness, and zinc spikes), coating integrity (no peeling or missing plating), impurity detection (no residual flux residue), and specific areas of zinc nodules and zinc ash. Inspection is conducted visually, tactilely, and under light to ensure a smooth surface, free of obvious defects, and complete coverage of the substrate. This inspection method quickly assesses the product's surface quality, ensuring both aesthetics and basic corrosion resistance. This is particularly important for areas that may affect performance or corrosion resistance. Only samples that meet all requirements are considered to meet appearance quality standards.

[0079] Interface bonding strength: The bonding strength test between the coating and the substrate is conducted in accordance with GB / T6396-2008 standard using a UTM5305 universal mechanical performance testing machine. The sample is cut along the coating direction, small squares are pre-cut on the coating surface, and then 1×10-3 s -1 The peel test is performed at a strain rate of 1000 nm. The bonding strength is calculated by recording the maximum peel force and dividing it by the pre-cut area, thereby evaluating the bonding quality between the coating and the substrate.

[0080] Corrosion Resistance: The corrosion resistance of the coating was tested using the double-cycle potentiodynamic reactivation (DL-EPR) method according to ASTM G108-94. Electrochemical testing was performed in a 0.5 mol / L H₂SO₄ + 0.01 mol / L KSCN solution at a scan rate of 1.5 mV / s. The corrosion resistance of the coating was evaluated by comparing the maximum current density ratio (Ir / Ia) in the forward and reverse scans, i.e., the reactivation rate (DOS%), providing an important reference for the coating's protective effectiveness.

[0081] Tensile Strength: The overall mechanical properties of hot-dip galvanized steel are evaluated through tensile testing. Samples are cut vertically into 75 mm x 4 mm specimens and tested using a universal testing machine. At a tensile rate of 1 mm / min, stress-strain curves are recorded while deformation and delamination of the coating are observed. By measuring parameters such as tensile strength and elongation at break, the mechanical properties of hot-dip galvanized steel are comprehensively evaluated.

[0082] The properties of the hot-dip galvanized steels of Examples 1 to 4 and Comparative Examples 1 to 4 are summarized in Table 1.

[0083] Table 1 Performance summary of hot-dip galvanized steel in Examples 1 to 4 and Comparative Examples 1 to 4

[0084] The main difference between Comparative Example 1 and Example 1 lies in the quenching temperature. As can be seen in Table 1, a higher quenching temperature (900°C) results in decreased interfacial bonding strength and tensile strength, while increasing the reactivation rate (DOS) and elongation. This is because the higher quenching temperature accelerates the diffusion of carbon atoms, promoting surface decarburization and forming a thicker decarburized layer (0.1 mm). The presence of the decarburized layer reduces the strength of the steel surface, thereby affecting the bonding strength between the coating and the substrate. At the same time, due to the reduced surface strength, the overall tensile strength of the material also decreases, but the ductility is improved. The thicker decarburized layer also leads to a decrease in surface corrosion resistance, thereby increasing the reactivation rate (DOS).

[0085] The main difference between Comparative Example 2 and Example 1 lies in the carbon potential of the heating atmosphere. As can be seen in Table 1, the lower carbon potential (0.06%) also leads to decreased interfacial bonding strength and tensile strength, while increasing the reactivation rate (DOS) and elongation. This is because the lower carbon potential increases the carbon concentration gradient between the steel surface and the surrounding atmosphere, promoting the outward diffusion of carbon atoms and exacerbating surface decarburization (forming a 0.11 mm thick decarburized layer). This more significant decarburization effect, similar to that in Comparative Example 1, leads to reduced surface strength, affecting the coating bonding strength and overall tensile properties. At the same time, decarburization reduces surface corrosion resistance, leading to an increase in the reactivation rate (DOS).

[0086] The main difference between Comparative Example 3 and Example 1 lies in the lower hot-dip galvanizing temperature (480°C). As shown in Table 1, the lower galvanizing temperature leads to a slight decrease in interfacial bonding strength, but slightly improves the reactivation rate (DOS). Tensile strength and elongation change little. This is because the lower temperature reduces the diffusion reaction between Fe and Zn, forming a thinner transition layer (15 μm). This thin transition layer slightly reduces the bonding strength between the coating and the substrate, but at the same time improves surface uniformity, thereby slightly improving corrosion resistance.

[0087] The main difference between Comparative Example 4 and Example 1 lies in the higher hot-dip galvanizing temperature (580°C). As shown in Table 1, the higher galvanizing temperature increases the interfacial bonding strength but slightly increases the reactivation rate (DOS). The tensile strength decreases slightly, while the elongation increases slightly. This is because the higher temperature accelerates the diffusion reaction between Fe and Zn, forming a thicker transition layer (83 μm). The thick transition layer strengthens the bonding strength between the coating and the substrate, but at the same time increases surface unevenness, which slightly reduces corrosion resistance. The higher galvanizing temperature also has a certain annealing effect on the substrate, resulting in a slight decrease in tensile strength and a slight increase in ductility.

[0088] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that any equivalent structural transformations made within the scope of the present invention using the contents of the present invention's description and drawings should be included within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing high-strength hot-dip galvanized steel, characterized in that: The following steps are involved: S1: cleaning carbon steel parts; the composition of the carbon steel parts is: C: 0.20-0.27%, B: 0.001-0.003%, Si: 0.02-0.06%, P: ≦0.020%, Cr: 0.10-0.20%, and the rest is Fe; S2: performing stepwise heating on the carbon steel part obtained in step S1 to slightly decarburize the surface of the carbon steel part, and then performing quenching treatment to obtain a quenched carbon steel part; S3: pickling and water washing the quenched carbon steel part obtained in step S2 in sequence, and performing a plating-assisting treatment using a plating-assisting solution; S4: immersing the carbon steel part obtained by the process in step S3 into a molten zinc solution for hot-dip galvanizing, and then sequentially performing centrifugal dezincification, water cooling, and discharging treatment to obtain the high-strength hot-dip galvanized steel.

2. The method for preparing high-strength hot-dip galvanized steel according to claim 1, characterized in that: In step S2, the process parameters of the step-by-step heating are: first, the temperature is increased from room temperature to 340-350°C at a rate of 1-5°C / min, then the temperature is increased to 550-560°C at a rate of 1-3°C / min, and then the temperature is increased to the quenching temperature at a rate of 0.5-1.5°C / min. The quenching temperature is 720-850°C. The heating atmosphere for the step-by-step heating is a mixed atmosphere of nitrogen and methanol; the carbon potential of the heating atmosphere is 0.08-0.12%.

3. The method for preparing high-strength hot-dip galvanized steel according to claim 2, characterized in that: In the step S2, the quenching liquid used in the quenching is a 2% by mass polyethylene glycol aqueous solution, and the temperature of the quenching liquid is 35-40° C.; The hardness of the quenched carbon steel part is greater than 40HRC, and the thickness of the surface micro-decarburization layer is 0.03-0.08mm.

4. The method for preparing high-strength hot-dip galvanized steel according to claim 1, characterized in that: In the step S3, the quenched carbon steel part obtained in step S2 is sequentially subjected to pickling, water washing and plating treatment within 1 hour after discharge; The pickling is carried out by using a pickling agent, and the pickling time is 4 to 6 minutes; the preparation method of the pickling agent comprises the following steps: adding ferrous chloride to hydrochloric acid with a mass fraction of 5 to 6%, stirring and mixing to obtain the pickling agent; the concentration of ferrous chloride in the pickling agent is 50 to 100 g / L; The plating-assisting solution is an aqueous solution containing 200-250 g / L ammonium chloride and 5-10 g / L zinc chloride, and the pH value of the plating-assisting solution is adjusted to 4-5 with hydrochloric acid; The temperature of the plating assist treatment is 30-40° C., and the time is 30-90 seconds.

5. The method for preparing high-strength hot-dip galvanized steel according to claim 1, characterized in that: In step S4, the composition of the molten zinc solution is: Fe: 0.2-0.35%, Ni: 0.030-0.045%, Al: 0.015-0.025%, and the rest is Zn; The temperature of the hot-dip galvanizing is 520-540° C., and the time is 25-35 seconds.

6. A high-strength hot-dip galvanized steel, characterized in that: The high-strength hot-dip galvanized steel is prepared by the preparation method described in any one of claims 1 to 5; The high-strength hot-dip galvanized steel comprises a carbon steel layer, a transition layer and a galvanized layer on the carbon steel layer, wherein the transition layer is located between the carbon steel layer and the galvanized layer, the thickness of the transition layer is 20-60 μm, and the thickness of the galvanized layer is 40-80 μm.

7. The high-strength hot-dip galvanized steel according to claim 6, characterized in that: The transition layer contains ζ-FeZn 13 ,δ-FeZn 10 and Fe2B; The transition layer contains ζ-FeZn 13 Form a lattice matching interface with Fe2B; The Fe2B columnar crystals in the transition layer present a tooth-like structure and are perpendicular to the transition layer interface; the average spacing of the Fe2B columnar crystals is 2-4 μm; The ζ-FeZn in the transition layer 13 and δ-FeZn 10 Evenly distributed between Fe2B columnar crystals.

8. The high-strength hot-dip galvanized steel according to claim 7, characterized in that: The α-Fe in the carbon steel layer and the Fe2B phase in the transition layer form a lattice matching interface.

9. Application of the high-strength hot-dip galvanized steel prepared by the preparation method as described in any one of claims 1 to 5 or the high-strength hot-dip galvanized steel as described in any one of claims 6 to 8 in grade 8 to grade 10 nut hot-dip galvanized layer fasteners.

Citation Information

Patent Citations

  • Heat treatment technology for reducing deformation of GCr15 thin-wall conical ring

    CN106048195A

  • Ultra-high strength hot-dip galvanized steel sheet having excellent surface quality and coating adhesion, and method for manufacturing thereof

    CN107002207A

  • Thermal forming member containing zinc coating layer and with tensile strength of grade 1800MPa and above and excellent cold bending property, and preparation method thereof

    CN110423945A

  • Hot-dip galvanizing method for low-alloy high-strength structural steel

    CN115896667A

  • High-strength cold-rolled hot-dip galvanized steel plate with high surface glossiness and manufacturing method thereof