Nitriding strengthening method for alloy surface layer, surface layer nitrided alloy and application of surface layer nitrided alloy
By forming a nitriding layer with a thickness of ≥2mm on the surface of the alloy substrate through plasma arc melting nitriding process, the problems of thin nitriding layer and increased brittleness in existing nitriding processes are solved, and the hardness and fatigue resistance of the alloy substrate are improved, making it suitable for high temperature, high speed and heavy load environments.
Patent Information
- Application Number
- CN202411025841.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-29
AI Technical Summary
Existing nitriding processes result in thinner nitrided layers and increased brittleness, failing to meet the surface hardness, wear resistance, and fatigue strength requirements of steel under harsh conditions.
Plasma arc nitriding is used to form a nitriding layer with a thickness of ≥2mm on the surface of the alloy substrate by controlling the plasma gas flow rate, current and moving speed, thus avoiding the formation of a white bright layer on the surface.
It significantly improves the surface hardness and fatigue resistance of the alloy substrate, extends its service life, and meets the requirements for use in high-temperature, high-speed, and heavy-load environments.
Smart Images

Figure CN118957485A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alloy surface strengthening, and in particular relates to a nitriding strengthening method for an alloy surface layer, a surface nitriding alloy and applications thereof. Background Art
[0002] With the rapid development of science and technology and economy, steel is used in harsh environments with high temperature, high speed and heavy load. The quality of steel has a decisive influence on the performance, life and reliability of mechanical equipment. Improving the surface hardness, fatigue resistance and corrosion resistance of steel and extending the service life of steel are the current key research directions and goals of steel. Steel with surface defects such as cracks, pits and scratches caused by steel production and processing also needs to be repaired through surface strengthening technology to further enhance the surface quality of steel.
[0003] In order to solve the problem of steel surface quality and improve the surface hardness and strength of steel, the surface of steel is often strengthened by surface nitriding, carburizing or surface coating. Among them, the surface nitriding process causes lattice distortion and improves the strength of steel by solid dissolving nitrogen atoms in the steel substrate. The fine and dispersed nitrogen-containing precipitates can refine the grains, hinder dislocation migration, and play a role in precipitation strengthening. The commonly used surface nitriding methods are nitriding furnace gas nitriding and glow discharge ion nitriding. In the above two nitriding processes, the diffusion coefficient of nitrogen in steel is low, resulting in a thin nitriding layer (generally about 200μm). During the nitriding process, a white bright layer is likely to be generated on the surface of the sample, resulting in an increase in the brittleness of the nitriding layer. During the use of steel, the surface hardness, wear resistance and fatigue strength decrease, which cannot meet the surface requirements of steel used under more harsh conditions. Summary of the invention
[0004] The object of the present invention is to provide a nitriding strengthening method for the surface layer of an alloy, a surface nitriding alloy and its application. The present invention adopts a plasma arc for melt nitriding to obtain a nitriding layer with a thickness of ≥2 mm on the surface of an alloy substrate, and no surface white bright layer is generated. The alloy substrate after nitriding strengthening has excellent hardness, wear resistance and fatigue strength.
[0005] In order to achieve the purpose of the present invention, the present invention provides the following technical solutions:
[0006] A method for nitriding strengthening of an alloy surface layer comprises the following steps:
[0007] The alloy substrate is melt-nitrided by plasma arc in a nitrogen atmosphere to obtain a nitrided layer on the surface of the alloy substrate; the thickness of the nitrided layer is ≥ 2 mm;
[0008] The parameters of the plasma arc include: the plasma gas is argon, the plasma gun gas flow rate is 5-15 L / min, the current is 120-180 A, and the plasma arc moving speed is 2-4 s / cm 2 .
[0009] Preferably, the pressure of the nitrogen atmosphere is 0.07-0.1 MPa; the nitrogen atmosphere is obtained by introducing nitrogen gas at a flow rate of 5-8 L / min.
[0010] Preferably, the vacuum is performed before the nitrogen is introduced; the vacuum degree of the vacuum is 1×10 -3 ~3×10 -3 Pa.
[0011] Preferably, the alloy substrate comprises steel or titanium alloy.
[0012] Preferably, the thickness of the nitriding layer is 2.0-3.0 mm.
[0013] Preferably, the method further comprises: grinding and cleaning the alloy substrate in sequence before the melt nitriding.
[0014] The present invention also provides a surface nitriding alloy, comprising an alloy substrate and a nitriding layer arranged on the surface of the alloy substrate; the thickness of the nitriding layer is ≥2mm; the nitriding layer is prepared by the nitriding strengthening method described in the above technical solution.
[0015] Preferably, the mass content of nitrogen in the surface nitriding alloy is 0.15-0.5%.
[0016] The present invention also provides the application of the surface nitriding alloy described in the above technical solution in automobile manufacturing or aerospace materials.
[0017] The present invention provides a nitriding strengthening method for an alloy surface layer, comprising the following steps: performing melt nitriding on an alloy substrate by using a plasma arc in a vacuum atmosphere and a nitrogen atmosphere, and obtaining a nitrided layer on the surface of the alloy substrate; the thickness of the nitrided layer is ≥2 mm; the parameters of the plasma arc include: the plasma gas is argon gas, the plasma gun gas flow rate is 5 to 15 L / min; the current is 120 to 180 A, and the plasma arc moving speed is 2 to 4 s / cm 2 The plasma arc melt nitriding of the present invention uses plasma as a heat source, instantly releasing high temperature (4000-6000°C) to melt the surface of the alloy substrate, and due to the high energy of the plasma arc (the energy density of the plasma arc is usually 1000-100000W / cm 2), the internal energy of nitrogen molecules increases after absorbing heat, and they instantly dissociate into nitrogen atoms. The diffusion coefficient in the melt increases, so that the nitrogen atoms melt into the melt. After the surface layer of the alloy substrate solidifies, the nitrogen concentration is much greater than the thermodynamic nitrogen saturation, and efficient nitriding is achieved on the surface of the alloy substrate. It can be seen from the results of the embodiments of the present invention that the thickness of the nitrided layer on the surface of the alloy substrate of the present invention is ≥2mm, which effectively improves the surface hardness and fatigue resistance of the alloy substrate, prolongs the service life of the alloy substrate, enhances the stability of the alloy substrate during use, and meets the requirements for the use of the alloy substrate in harsh environments such as high temperature, high speed, and heavy load. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0019] Figure 1 This is the structure diagram of the plasma furnace;
[0020] Figure 2 A schematic diagram of the nitriding strengthening method for the alloy surface layer of the present invention;
[0021] Figure 3 This is a flow chart of the nitriding strengthening method for the alloy surface layer of Example 1 of the present invention;
[0022] Figure 4 This is a comparison chart of the effects of the nitriding strengthening method for the alloy surface layer in Example 1 of the present invention and nitriding furnace gas nitriding and glow discharge ion nitriding. DETAILED DESCRIPTION
[0023] The present invention provides a nitriding strengthening method for an alloy surface layer, comprising the following steps:
[0024] The alloy substrate is melt-nitrided by plasma arc in a nitrogen atmosphere to obtain a nitrided layer on the surface of the alloy substrate; the thickness of the nitrided layer is ≥ 2 mm;
[0025] The parameters of the plasma arc include: the plasma gas is argon, the plasma gun gas flow rate is 5-15 L / min; the current is 120-180 A, and the plasma arc moving speed is 2-4 s / cm 2 .
[0026] In the present invention, unless otherwise specified, all raw materials are preferably commercially available products well known to those skilled in the art.
[0027] In the present invention, the alloy substrate preferably includes steel or titanium alloy, more preferably steel; the steel includes high-quality steel or plain carbon steel; the high-quality steel is preferably M50 bearing steel or 440C steel; the mass content of nitrogen in the high-quality steel is preferably 0.005-0.10%, more preferably 0.0073-0.0082%.
[0028] In the present invention, the pressure of the nitrogen atmosphere is preferably 0.07 to 0.1 MPa, more preferably 0.08 to 0.09 MPa; the nitrogen filling flow rate in the nitrogen atmosphere is preferably 5 to 8 L / min, more preferably 6 to 7 L / min.
[0029] In the present invention, the melt nitriding is preferably performed under vacuum; the vacuum degree of the vacuum is preferably 1×10 -3 ~3×10 -3 Pa, more preferably 2×10 -3 Pa; the vacuum method preferably includes: using a mechanical pump to reduce the vacuum degree in the furnace to less than 300Pa, starting a Roots pump, and after the vacuum degree is reduced to 1Pa, starting a diffusion pump until the vacuum degree in the furnace is 1×10 -3 ~3×10 -3 Pa.
[0030] In the present invention, the parameters of the plasma arc include: the plasma gas is argon, the plasma gun gas flow rate is 5 to 15 L / min, preferably 10 to 12 L / min; the current is 120 to 180 A, preferably 140 to 160 A; the plasma arc moving speed is 2 to 4 s / cm 2 , preferably 3s / cm 2 .
[0031] In the present invention, it is also preferred to grind and clean the alloy substrate in sequence, and the present invention has no special limitation on the grinding; the cleaning reagent preferably includes ethanol and acetone; and the ethanol is preferably anhydrous ethanol.
[0032] The plasma arc melt nitriding of the present invention uses plasma as a heat source, instantly releasing high temperature (4000-6000°C) to melt the surface of the alloy substrate, and due to the high energy of the plasma arc (the energy density of the plasma arc is usually 1000-100000W / cm 2), the internal energy of nitrogen molecules increases after absorbing heat, and the nitrogen molecules in the plasma furnace instantly dissociate into nitrogen atoms. The diffusion coefficient in the melt increases, causing the nitrogen atoms to melt into the melt. After the surface of the alloy substrate solidifies, the nitrogen concentration is much greater than the thermodynamic nitrogen saturation, and efficient nitriding is achieved on the surface of the alloy substrate. Compared with carbon, nitrogen is more likely to preferentially combine with Cr, Mo, and V in the alloy melt to exist in the steel in the form of solid solution, or to generate fine dispersed carbon-nitrogen composite precipitates uniformly distributed in the steel, thereby inhibiting the formation of large-sized, irregular and aggregated carbides during the solidification of the molten steel. For example, during the nitrogen melting process of steel, nitrogen and carbon elements are solid-solution strengthened, and the precipitates in the steel are transformed. After the surface of the steel is molten nitrided, the cooling gradient is large, and the structure in the steel is transformed into martensite. The bonding force between the molten nitrided layer and the steel is strong. Moreover, due to the rapid re-solidification after the plasma arc dissolving nitrogen, it was found under the scanning electron microscope that the carbides in the nitrided layer basically disappeared, and there was obvious stratification between the nitrided layer and the substrate, which can greatly enhance the surface hardness and fatigue resistance of the substrate and extend the service life of high-quality steel.
[0033] The present invention also provides a surface nitriding alloy, comprising an alloy substrate and a nitriding layer arranged on the surface of the alloy substrate; the nitriding layer is prepared by the nitriding strengthening method described in the above technical solution.
[0034] In the present invention, the phase composition of the nitriding layer preferably includes Fe2N, Fe3N and FeN 0.076 phase; the thickness of the nitriding layer is ≥2mm, preferably 2.44~2.51mm, more preferably 2.48mm; the mass content of nitrogen in the surface nitriding alloy is preferably 0.15~0.5%, more preferably 0.159~0.416%, further preferably 0.192~0.273%.
[0035] The present invention also provides the application of the surface nitriding alloy described in the above technical solution in automobile manufacturing or aerospace materials.
[0036] In order to further illustrate the present invention, a nitriding strengthening method for an alloy surface layer, a surface nitriding alloy and applications thereof provided by the present invention are described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0037] Example 1
[0038] M50 bearing steel (nitrogen content of 0.0073%) was processed into a sample with a size of 200×150×15 mm by wire cutting. The surface of the sample was polished with sandpaper, cleaned with anhydrous ethanol and acetone in turn, and then placed in Figure 1 In the plasma furnace shown;
[0039] according to Figure 2 The schematic diagram and Figure 3The flow chart performs nitriding strengthening on the alloy surface, and the specific steps are:
[0040] Preparation of vacuum and nitrogen atmosphere in plasma furnace: The vacuum system is a three-stage pump: mechanical pump, Roots pump, and diffusion pump. First, start the mechanical pump. When the vacuum degree in the furnace is less than 300Pa, start the Roots pump. When the vacuum degree continues to decrease to 1Pa, start the diffusion pump again until the vacuum degree in the furnace reaches 3×10 -3 Pa; After the vacuum preparation is completed, high-purity nitrogen is filled into the furnace at a flow rate of 5L / min until the pressure in the furnace reaches 0.0.08MPa;
[0041] Plasma arc was used for melt nitriding. The plasma arc parameters were set as follows: argon plasma gun gas was 10 L / min, and the plasma arc moving speed was 2 s / cm 2 , the currents are 120A, 140A and 160A respectively.
[0042] The performance of the surface nitrided M50 bearing steel of Example 1 was tested, wherein the wear test environment was 350°C high temperature wear, and the corrosion performance test environment was an electrochemical test in a 3.5% NaCl solution. The test results are shown in Table 1.
[0043] Table 1 Performance test results of surface nitrided steel in Example 1
[0044]
[0045] It can be seen from the results in Table 1 that the nitrogen content of the surface layer of the bearing steel is increased after the plasma arc nitriding of the present invention, and the thickness of the nitriding layer is 2.44-2.51 mm. In terms of mechanical properties, the hardness of the original M50 bearing steel is 241HV0.02. After nitriding under different currents, it is increased to 738HV0.02, 778HV0.02 and 759HV0.02 respectively. The hardness of the nitriding layer surface to the substrate decreases as a whole. The surface and subsurface hardness strengthening effect of the bearing steel after nitriding with 140A current is the most significant; compared with the original bearing steel sample, as the nitrogen content of the surface layer of the bearing steel increases, the average wear coefficient decreases by about 7%, 16%, and 32%, respectively, the wear volume decreases by about 44%, 53%, and 69%, respectively, and the volume wear rate decreases by about 47%, 56%, and 70%, respectively. The corrosion potential increases by 13%, 18%, and 35%, respectively, and the corrosion current density decreases by 25%, 29%, and 35%, respectively.
[0046] Figure 4 The present invention implements the nitriding strengthening method of the alloy surface 1 and the effect comparison diagram of nitriding furnace gas nitriding and glow discharge ion nitriding, by Figure 4 It can be seen that compared with nitriding furnace gas nitriding and glow discharge ion nitriding, the thickness and sub-surface strengthening distance of the alloy surface layer in the nitriding strengthening method of the present invention are greatly increased, and it has a better nitriding effect.
[0047] Example 2
[0048] 440C steel (nitrogen content 0.0082%) was processed into samples with a size of 200×150×15 mm by wire cutting. The surface of the sample was polished with sandpaper, cleaned with anhydrous ethanol and acetone in turn, and then placed in a plasma furnace;
[0049] Preparation of vacuum and nitrogen atmosphere in plasma furnace: The vacuum system is a three-stage pump: mechanical pump, Roots pump, and diffusion pump. First, start the mechanical pump. When the vacuum degree in the furnace is less than 300Pa, start the Roots pump. When the vacuum degree continues to decrease to 1Pa, start the diffusion pump again until the vacuum degree in the furnace reaches 3×10 -3 Pa; After the vacuum preparation is completed, high-purity nitrogen is filled into the furnace at a flow rate of 5L / min until the pressure in the furnace reaches 0.0.08MPa;
[0050] Plasma arc was used for melt nitriding. The plasma arc parameters were set as follows: argon plasma gun gas was 10 L / min, currents were 120 A, 140 A and 160 A respectively, and the plasma arc moving speed was 2 s / cm 2 .
[0051] The performance of the surface nitrided M50 bearing steel of Example 2 was tested, and the test results are shown in Table 2.
[0052] Table 2 Performance test results of surface nitrided steel in Example 2
[0053]
[0054] From the results in Table 2, it can be seen that after nitriding with different plasma arc currents of 120A, 140A, and 160A, the nitrogen content of the surface layer of 440C steel increased to 0.152%, 0.155%, and 0.192%, respectively. In terms of mechanical properties, the hardness of the original 440C steel was 223HV0.02, and after nitriding under different parameters, it increased to 457HV0.02, 515HV0.02, and 546HV0.02, respectively. The hardness of the nitrided layer surface to the substrate decreased gradually in the range of 1 to 3mm. After nitriding with a current of 160A, the surface and subsurface hardness of the sample were strengthened most significantly.
[0055] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for nitriding strengthening of an alloy surface, characterized in that: The following steps are involved: The alloy substrate is melt-nitrided by plasma arc in a nitrogen atmosphere to obtain a nitrided layer on the surface of the alloy substrate; the thickness of the nitrided layer is ≥ 2 mm; The parameters of the plasma arc include: the plasma gas is argon, the plasma gun gas flow rate is 5-15 L / min, the current is 120-180 A, and the plasma arc moving speed is 2-4 s / cm 2 .
2. The nitriding strengthening method according to claim 1, characterized in that: The pressure of the nitrogen atmosphere is 0.07-0.1 MPa; the nitrogen atmosphere is obtained by introducing nitrogen gas, and the nitrogen gas charging flow rate is 5-8 L / min.
3. The nitriding strengthening method according to claim 1, characterized in that: The vacuum is performed before the nitrogen is introduced; the vacuum degree of the vacuum is 1×10 -3 ~3×10 -3 Pa.
4. The nitriding strengthening method according to claim 1, characterized in that: The alloy substrate comprises steel or titanium alloy.
5. The nitriding strengthening method according to claim 1, characterized in that: The thickness of the nitriding layer is 2.0-3.0 mm.
6. The nitriding strengthening method according to claim 1, characterized in that: Also includes: Before the melt nitriding, the alloy substrate is polished and cleaned in sequence.
7. A surface nitriding alloy, characterized in that: It comprises an alloy substrate and a nitriding layer arranged on the surface of the alloy substrate; the thickness of the nitriding layer is ≥2mm; the nitriding layer is prepared by the nitriding strengthening method according to any one of claims 1 to 6.
8. The surface nitriding alloy according to claim 7, characterized in that: The mass content of nitrogen in the surface nitriding alloy is 0.15-0.5%.
9. Use of the surface nitriding alloy according to claim 7 or 8 in automobile manufacturing or aerospace materials.
Citation Information
Patent Citations
Compound reinforcement treating method for surface energy carrying beam of nitriding steel
CN105463383A
Plasma corrosion resistant part, preparation method thereof and plasma processing equipment
CN113522688A
Method for ion-plasma nitriding of parts from tool steel
RU2599950C1
Substrate of improved plasma sprayed surface morphology and its use as an electrode in an electrolytic cell