TiAlN / AlTiN / ZrN coated cutting tool with composite multilayer structure and preparation method of TiAlN / AlTiN / ZrN coated cutting tool

By adopting a composite multi-layer TiAlN/AlTiN/ZrN coating on the titanium alloy cutting tool, combined with physical vapor deposition technology and alternating arrangement of the combined layer, the problem of easy failure of the titanium alloy cutting tool coating is solved, and the tool is significantly improved cutting life and wear resistance.

CN118957492AActive Publication Date: 2024-11-15JIANGSU TIANGONG CEMENTED CARBIDE TECH CO LTD

Patent Information

Application Number
CN202411040436.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The existing titanium alloy cutting tool coating is prone to failure, resulting in insufficient tool life.

Method used

TiAlN/AlTiN/ZrN coating tool with composite multilayer structure is used to coat multilayer materials, including TiAlN, AlTiN and ZrN layers, combining alternating arrangement of layers and optimizing process parameters to improve coating bonding and wear resistance.

Benefits of technology

It improves the high temperature resistance, oxidation resistance and binding force of the coating, extends the cutting life of the tool, avoids the peeling and film delamination of the coating, reduces the friction coefficient, and enhances the wear resistance and cutting performance of the tool.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957492A_ABST
    Figure CN118957492A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of metal cutting tools, in particular to a TiAlN / AlTiN / ZrN coating tool of a composite multilayer structure and a preparation method. The TiAlN / AlTiN / ZrN coated cutting tool with the composite multilayer structure comprises a base material and a plurality of material layers plated on the surface of the base material through a PVD (Physical Vapor Deposition) process, and the first material layer is a TiAlN layer; the second material layer is an AlTiN layer; the third material layer is a ZrN layer; the fourth material layer is an AlTiN layer; the fifth material layer is a ZrN layer; the sixth material layer is an AlTiN layer; the seventh material layer is a ZrN layer, the coating binding force of the seventh material layer is 108 N, the nano hardness is 33.43 GPa, the cutting force is 73 N, the rear tool face abrasion loss is 0.12 mm, high strength and toughness are achieved, the binding force is high, and the cutting life of the coated tool is far longer than that of a traditional AlTiN coated tool.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal cutting tools, and in particular to a TiAlN / AlTiN / ZrN coating tool with a composite multilayer structure and a preparation method thereof. Background Art

[0002] Titanium alloy materials have been widely used in aerospace, medical, 3C and other fields due to their excellent properties such as light weight, high strength and corrosion resistance, but the good material properties also bring difficulties to their processing. The increasingly widespread application of titanium alloys has led to an increasing market demand for coatings for titanium alloy cutting tools.

[0003] There are many studies on titanium alloy machining coatings. One of them is to use physical vapor deposition technology (PVD) to coat the tool surface with TiAlN coating materials with high hardness, high chemical stability, low friction, wear resistance, and high temperature resistance to improve cutting efficiency and extend cutting life.

[0004] In order to further improve the performance of the coating, an AlTiN high-hardness coating will be coated on the basis of the TiAlN coating, and the high-hardness Al2O3 content will be increased through the coating with a high Al content. Patent technical document CN202310021859.X discloses a multi-structure heterogeneous coating and its preparation method and application, which includes a TiAlN bottom layer, an AlTiN gradient layer with increasing Al content, an AlTiN / TiSiN nano-multilayer and a TiSiN nano-composite layer connected in sequence. The coating has strong and corrosion-resistant properties and high bonding strength. The cutting life of its coated tool is much longer than that of traditional AlTiN coated tools, but the high-hardness AlTiN coating still has a large internal stress, which will affect the service life of the coated tool in actual application. Summary of the invention

[0005] In view of this, the purpose of the present invention is to propose a composite multilayer structure TiAlN / AlTiN / ZrN coated tool and a preparation method to solve the problem of insufficient tool life caused by easy failure of titanium alloy cutting tool coating in the prior art.

[0006] Based on the above purpose, the present invention provides a TiAlN / AlTiN / ZrN coated tool with a composite multilayer structure, comprising a base material and a multilayer material layer plated on the surface of the base material by a PVD process, wherein the first material layer is a TiAlN layer; the second material layer is an AlTiN layer; the third material layer is a ZrN layer; the fourth material layer is an AlTiN layer; the fifth material layer is a ZrN layer; the sixth material layer is an AlTiN layer; and the seventh material layer is a ZrN layer.

[0007] Preferably, the first material layer includes a plurality of stacked bonding layers, namely a first bonding layer, a second bonding layer and a third bonding layer.

[0008] Preferably, the thickness of the first material layer is between 1.0 and 1.2 μm, and the thickness of the second material layer is between 0.8 and 1.0 μm.

[0009] Furthermore, the present invention also provides a method for preparing a TiAlN / AlTiN / ZrN coated tool with a composite multilayer structure, and the specific preparation steps are as follows:

[0010] (1) Place the substrate material in the vacuum coating equipment and adjust the vacuum degree of the equipment to 8×10 -5 mbar, heating for 60 min, so that the temperature rises to 460-480°C;

[0011] (2) using a PVD process to plate a first material layer on the base material, wherein the first material layer is a TiAlN layer;

[0012] (3) using a PVD process to plate a second material layer on a side of the first material layer away from the base material, wherein the second material layer is an AlTiN layer;

[0013] (4) using a PVD process to plate a third material layer on a side of the second material layer away from the base material, wherein the third material layer is a ZrN layer;

[0014] (5) using a PVD process to plate a fourth material layer on a side of the third material layer away from the base material, wherein the fourth material layer is an AlTiN layer;

[0015] (6) using a PVD process to plate a fifth material layer on a side of the fourth material layer away from the base material, wherein the fifth material layer is a ZrN layer;

[0016] (7) using a PVD process to plate a sixth material layer on a side of the fifth material layer away from the base material, wherein the sixth material layer is an AlTiN layer;

[0017] (8) A seventh material layer is plated on a side of the sixth material layer away from the base material using a PVD process, wherein the seventh material layer is a ZrN layer.

[0018] Preferably, the base material in step (1) is cemented carbide.

[0019] Preferably, in step (2), the first material layer comprises a plurality of stacked bonding layers, and the specific preparation steps are as follows: each bonding layer is plated in turn by a PVD process. When a single bonding layer is plated, the TiAl target is placed at a molecular pump frequency of 72% and a pressure of 2.5×10 -1The target material is processed in a nitrogen environment with an arc current of 150A, a bias voltage of a preset voltage, a temperature of 480°C for a preset time, an N2 flow rate of 1200SCCM, and a material ratio of Ti to Al in the TiAl target material of 50 / 50. The closer the bonding layer is to the second material layer, the greater the bias voltage required during coating.

[0020] Preferably, when the first bonding layer is plated on the base material using the PVD process, the required bias voltage is 40V and the processing time is 40±2min; when the second bonding layer is plated on the base material, the required bias voltage is 80V and the processing time is 2min; when the third bonding layer is plated on the base material, the required bias voltage is 120V and the processing time is 30±2min.

[0021] Preferably, the method for coating the second material layer in step (3) is: placing the TiAl target and the Al target at a molecular pump frequency of 72% and a pressure of 2.5×10 -1 The second material layer can be obtained on the substrate material by treating it in a nitrogen environment with an arc current of 150A, a bias voltage of 80V and a temperature of 480°C for 2min. The N2 flow rate is 1200SCCM, wherein the amount of Ti and Al in the TiAl target is 50 / 50.

[0022] Preferably, the method for coating the third material layer in step (4) is: placing the Zr target material in a molecular pump with a frequency of 72% and a pressure of 2.5×10 -1 The third material layer can be obtained on the substrate material by treating it in a nitrogen environment with an arc current of 150A, a bias voltage of 120V and a temperature of 480°C for 30min, and the N2 flow rate is 1200SCCM.

[0023] Preferably, the method of plating the AlTiN layer by using the PVD process in steps (4) and (6) is the same as that in step (2); and the method of plating the ZrN layer by using the PVD process in steps (3) and (5) is the same as that in step (3).

[0024] Beneficial effects of the present invention:

[0025] (1) The coated tool obtained by plating the ZrN layer by PVD process in the present invention has low affinity with the processed material (titanium alloy). The low affinity makes the tool wear in the form of abrasive wear during cutting, and the coating is not easily carried away by the abrasive particles.

[0026] (2) The AlTiN layer coated tool obtained by the PVD process of the present invention has excellent high temperature resistance, red hardness and oxidation resistance, which makes the coating have a longer service life, improves the wear resistance and bonding strength of the coating, makes the coating less likely to fail, avoids coating peeling, and improves the cutting life of the tool.

[0027] (3) The present invention adopts the PVD process to alternately plate AlTiN layers and ZrN layers to obtain a coated tool, so that AlTiN and ZrN have excellent bonding strength, ensuring that no film peeling occurs during the tool cutting process, and at the same time brings a low friction coefficient. The low friction coefficient is beneficial to reducing the heat generated by the friction between the tool and the processed material, thereby reducing the heat extended to the base material. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0029] Figure 1 A partial enlarged cross-sectional view of a tool prepared according to an embodiment of the present invention;

[0030] Figure 2 This is an EDS analysis diagram of the coating of the tool prepared in the embodiment of the present invention;

[0031] The markings in the figure are:

[0032] 1. Base material; 2. First material layer TiAlN coating; 3. Second material layer AlTiN coating; 4. Third material layer ZrN coating; 5. Fourth material layer AlTiN coating; 6. Fifth material layer ZrN coating; 7. Sixth material layer AlTiN coating; 8. Seventh material layer ZrN coating. DETAILED DESCRIPTION

[0033] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0034] As shown in the figure, this embodiment discloses a TiAlN / AlTiN / ZrN coated tool with a composite multilayer structure, including a base material 1, and the base material is cemented carbide. Specifically, the base material 1 of this embodiment is used for cemented carbide and high-speed steel tools, including blades, milling cutters, drill bits, reamers, etc. The outer side of the base material is plated with a first material layer 2 using a PVD process, and the first material layer is a TiAlN layer. The first material layer also includes three bonding layers (not shown in the figure), and the thickness of the first material layer is between 1.0 and 1.2 μm; a second material layer 3 is plated on the side of the first material layer 2 away from the base material using a PVD process, and the second material layer 3 is an AlTiN layer, and the thickness of the second material layer 3 is between 0.8 and 1.0 μm; a third material layer 4 is plated on the side of the second material layer 3 away from the base material using a PVD process, and the third material layer 4 It is a ZrN layer; a fourth material layer 5 is plated on the side of the third material layer 4 away from the base material by using the PVD process, and the fourth material layer 5 is an AlTiN layer; a fifth material layer 6 is plated on the side of the fourth material layer 5 away from the base material by using the PVD process, and the fifth material layer 6 is a ZrN layer; a sixth material layer 7 is plated on the side of the fifth material layer 6 away from the base material by using the PVD process, and the sixth material layer 7 is an AlTiN layer; a seventh material layer 8 is plated on the side of the sixth material layer 7 away from the base material by using the PVD process, and the seventh material layer 8 is a ZrN layer.

[0035] Embodiment: A method for preparing a composite multilayer structure TiAlN / AlTiN / ZrN coated tool comprises the following steps:

[0036] (1) Place the cemented carbide in a vacuum coating device and adjust the vacuum degree of the device to 8×10 -5 mbar, heating for 60 min, so that the temperature rises to 470 ° C;

[0037] (2) using a PVD process to plate a first material layer on the cemented carbide, wherein the first material layer is a TiAlN layer;

[0038] (3) using a PVD process to plate a second material layer on a side of the first material layer away from the cemented carbide, wherein the second material layer is an AlTiN layer;

[0039] (4) using a PVD process to plate a third material layer on a side of the second material layer away from the cemented carbide, wherein the third material layer is a ZrN layer;

[0040] (5) using a PVD process to plate a fourth material layer on a side of the third material layer away from the cemented carbide, wherein the fourth material layer is an AlTiN layer;

[0041] (6) using a PVD process to plate a fifth material layer on a side of the fourth material layer away from the cemented carbide, wherein the fifth material layer is a ZrN layer;

[0042] (7) using a PVD process to plate a sixth material layer on a side of the fifth material layer away from the cemented carbide, wherein the sixth material layer is an AlTiN layer;

[0043] (8) A seventh material layer is plated on a side of the sixth material layer away from the cemented carbide by using a PVD process, wherein the seventh material layer is a ZrN layer.

[0044] In step (2), the first material layer includes a plurality of stacked bonding layers, and the specific preparation steps are as follows: each bonding layer is plated in turn by a PVD process. When a single bonding layer is plated, the TiAl target is placed in a molecular pump with a frequency of 72% and a pressure of 2.5×10 -1 mbar, arc striking current of 150A, bias voltage of preset voltage, temperature of 480°C in a nitrogen environment for preset time, N2 flow rate of 1200SCCM, the amount ratio of Ti to Al in the TiAl target material of 50 / 50, wherein, when the first bonding layer is plated on the base material by PVD process, the required bias voltage is 40V, and the processing time is 40; when the second bonding layer is plated on the base material, the required bias voltage is 80V, and the processing time is 2min; when the third bonding layer is plated on the base material, the required bias voltage is 120V, and the processing time is 30min.

[0045] The method for coating the second material layer in step (3) is to place the TiAl target and the Al target respectively in a molecular pump with a frequency of 72% and a pressure of 2.5×10 -1 The second material layer can be obtained on the substrate material by treating it in a nitrogen environment with an arc current of 150A, a bias voltage of 80V and a temperature of 480°C for 2min. The N2 flow rate is 1200SCCM, wherein the amount of Ti and Al in the TiAl target is 50 / 50.

[0046] The method for coating the third material layer in step (4) is to place the Zr target material in a molecular pump with a frequency of 72% and a pressure of 2.5×10 -1 The third material layer can be prepared on the base material by treating the substrate in a nitrogen environment with an arc current of 150A, a bias voltage of 120V and a temperature of 480°C for 30 minutes, wherein the N2 flow rate is 1200SCCM.

[0047] The method of plating the AlTiN layer in step (5) and step (7) is the same as the method of plating the AlTiN layer in step (3).

[0048] The method of plating the AlTiN layer in step (6) and step (8) is the same as the method of plating the AlTiN layer in step (4).

[0049] At the same time, it should be noted that the present invention is not simply combining TiAlN, AlTiN and ZrN together. The content of this patent application is a tool coating developed for processing titanium alloy materials. The selected coating structure and target material fully consider the processing characteristics of titanium alloy, and the coating has been strictly tested internally. Specifically, the effect of combining different target materials (structures) is affected by many factors, such as deposition temperature, magnetic field parameters, cathode, bias voltage, gas flow ion source, etc. Different parameters produce completely different effects.

[0050] The difficulty of combining AlTiN and ZrN lies in the following three points: first, to obtain excellent bonding strength between AlTiN and ZrN to ensure that there is no film peeling during tool cutting; second, to reduce the droplets of arc-deposited AlTiN and ZrN and reduce the friction coefficient by optimizing process parameters; third, to control the deposition time of each layer of coating to obtain the optimal combination of cutting edge sharpness, low friction coefficient and coating wear resistance while ensuring that the tool cutting edge does not peel off.

[0051] A series of performance tests were performed on the coated tools obtained in the examples:

[0052] The coating bonding force is measured by scratch method. In this experiment, an automatic scratch tester is used for scratch test. The force loading speed is 100N / m, the scratch length is 5mm, and the end load is 100N. The nanohardness is measured by UNHT nanoindenter, and the setting parameters are as follows: maximum load 10mN, loading rate 20mN / min, unloading rate 20mN / min, and holding time 10s. The cutting force is measured by Swiss Kistler 9257B force measuring equipment with a cutting speed of 105m / min. The measurement standard is that each set of blades is measured twice continuously under each set of cutting parameters, and the distance of each cutting is L=110mm. The wear resistance is carried out on the CK6140 horizontal lathe produced by Chongqing Honggang CNC Machine Tool Co., Ltd. The experimental standard is that each set of blades is continuously cut for 220mm at 105m / min until the cutting distance is L=2200mm, and the wear of the back face is measured.

[0053] The test results are as follows:

[0054] The coating tool of the present invention has a coating bonding force of 108N, a nano hardness of 33.43GPa, a cutting force of 73N, a back tool wear of 0.12mm, high strength and high toughness, and high bonding force. The cutting life of the coated tool is much longer than that of the traditional AlTiN coated tool.

[0055] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

[0056] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A composite multilayer structure TiAlN / AlTiN / ZrN coated tool, characterized in that: It comprises a base material and a multi-layer material layer plated on the surface of the base material by a PVD process, wherein the first material layer is a TiAlN layer; the second material layer is an AlTiN layer; the third material layer is a ZrN layer; and the fourth material layer is an AlTiN layer; The fifth material layer is a ZrN layer; the sixth material layer is an AlTiN layer; The seventh material layer is a ZrN layer.

2. The composite multilayer structure TiAlN / AlTiN / ZrN coated tool according to claim 1, characterized in that: The first material layer includes a plurality of stacked bonding layers, namely a first bonding layer, a second bonding layer and a third bonding layer.

3. The composite multilayer structure TiAlN / AlTiN / ZrN coated tool according to claim 1, characterized in that: The thickness of the first material layer is between 1.0 and 1.2 μm, and the thickness of the second material layer is between 0.8 and 1.0 μm.

4. A method for preparing a composite multilayer structure TiAlN / AlTiN / ZrN coated tool according to claims 1-3, characterized in that: The specific preparation steps are as follows: (1) Place the substrate material in the vacuum coating equipment and adjust the vacuum degree of the equipment to 8×10 -5 mbar, heated for 1h, so that the temperature rises to 460-480℃; (2) using a PVD process to plate a first material layer on the base material, wherein the first material layer is a TiAlN layer; (3) using a PVD process to plate a second material layer on a side of the first material layer away from the base material, wherein the second material layer is an AlTiN layer; (4) using a PVD process to plate a third material layer on a side of the second material layer away from the base material, wherein the third material layer is a ZrN layer; (5) using a PVD process to plate a fourth material layer on a side of the third material layer away from the base material, wherein the fourth material layer is an AlTiN layer; (6) using a PVD process to plate a fifth material layer on a side of the fourth material layer away from the base material, wherein the fifth material layer is a ZrN layer; (7) using a PVD process to plate a sixth material layer on a side of the fifth material layer away from the base material, wherein the sixth material layer is an AlTiN layer; (8) A seventh material layer is plated on a side of the sixth material layer away from the base material using a PVD process, wherein the seventh material layer is a ZrN layer.

5. The method for preparing a composite multilayer structure TiAlN / AlTiN / ZrN coated tool according to claim 4, characterized in that: The base material in step (1) is cemented carbide.

6. The method for preparing a composite multilayer structure TiAlN / AlTiN / ZrN coated tool according to claim 4, characterized in that: In step (2), the first material layer includes a plurality of stacked bonding layers, and the specific preparation steps are as follows: each bonding layer is plated in turn by a PVD process. When a single bonding layer is plated, the TiAl target is placed in a molecular pump with a frequency of 72% and a pressure of 2.5×10 -1 The target material is processed in a nitrogen environment with an arc current of 150A, a bias voltage of a preset voltage, a temperature of 480°C for a preset time, an N2 flow rate of 1200SCCM, and a material ratio of Ti to Al in the TiAl target material of 50 / 50. The closer the bonding layer is to the second material layer, the greater the bias voltage required during coating.

7. The method for preparing a composite multilayer structure TiAlN / AlTiN / ZrN coated tool according to claim 6, characterized in that: When the first bonding layer is plated on the base material using the PVD process, the required bias voltage is 40V and the processing time is 40±2min; when the second bonding layer is plated on the base material, the required bias voltage is 80V and the processing time is 2min; when the third bonding layer is plated on the base material, the required bias voltage is 120V and the processing time is 30±2min.

8. The method for preparing a composite multilayer structure TiAlN / AlTiN / ZrN coated tool according to claim 4, characterized in that: The method for coating the second material layer in step (3) is: placing the TiAl target and the Al target at a molecular pump frequency of 72% and a pressure of 2.5×10 -1 The second material layer can be obtained on the substrate material by treating it in a nitrogen environment with an arc current of 150A, a bias voltage of 80V and a temperature of 480°C for 2min. The N2 flow rate is 1200SCCM, wherein the amount ratio of Ti to Al in the TiAl target is 50 / 50.

9. The method for preparing a composite multilayer structure TiAlN / AlTiN / ZrN coated tool according to claim 4, characterized in that: The method for coating the third material layer in step (4) is: placing the Zr target material in a molecular pump with a frequency of 72% and a pressure of 2.5×10 -1 The third material layer can be obtained on the substrate material by treating it in a nitrogen environment with an arc current of 150A, a bias voltage of 120V and a temperature of 480°C for 30min, and the N2 flow rate is 1200SCCM.

10. The method for preparing a composite multilayer structure TiAlN / AlTiN / ZrN coated tool according to claim 4, characterized in that: The method of plating the AlTiN layer by PVD process in steps (5) and (7) is the same as that in step (3); the method of plating the ZrN layer by PVD process in steps (6) and (8) is the same as that in step (4).

Citation Information

Patent Citations

  • Multi-structure heterogeneous coating as well as preparation method and application thereof

    CN116411244A

  • Ti-Zr / ZrN nanometer multilayer coating cutter and preparation process thereof

    CN102181835A

  • Coated cutting tool with multi-layer structure and preparation method

    CN118291919A

  • Apparatus for manufacturing display device

    KR1020250022271A

Cited By

  • High-toughness high-wear-resistance Ti (C, N)-based metal ceramic material and preparation method thereof