Friction stir process for improving performance of laser metal deposition TC4 alloy
The laser-deposited TC4 titanium alloy is processed through the friction stir process, which solves the problems of cracks, pores and poor morphology during laser deposition, and improves the mechanical properties and processing efficiency of titanium alloys, and is environmentally friendly and has low cost. .
Patent Information
- Application Number
- CN202411070653.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-15
AI Technical Summary
During laser metal deposition, titanium alloys are prone to cracks, pores and poor morphology, resulting in poor quality of the cladding layer, which limits its application.
The friction stirring process is used to process the deposited TC4 titanium alloy. The friction heat is generated through the rotation and movement of the stirring head, and the workpiece is heated evenly, the temperature gradient is reduced, the thermal stress is reduced, and the heat input is controlled by controlling the stirring parameters to eliminate defects and residues. Stress to achieve grain refinement.
Effectively eliminate defects in the tissue, improve the mechanical properties of titanium alloys, enhance their wear resistance and corrosion resistance, reduce costs, and achieve efficient and rapid processing with green and environmental protection.
Smart Images

Figure CN118957570A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal processing, and in particular relates to a friction stirring process for improving the performance of laser metal deposition TC4 alloy. Background Art
[0002] Titanium alloys are difficult to process traditionally due to their high strength and low thermal conductivity. Laser metal deposition technology for manufacturing titanium alloys has brought many opportunities, but there are still some problems that need to be solved in practical applications.
[0003] The most prominent problem is the defects such as cracks, pores and poor morphology, which not only affect the quality of the cladding layer, but also restrict the wide application of laser cladding technology on the surface of titanium alloy.
[0004] High-power laser beams generate large residual stresses in the process of rapidly heating and cooling the substrate and cladding materials. This residual stress is the main cause of cracking in the cladding layer. Secondly, the formation of pores is also a problem that needs attention. During the laser cladding process, if the gas in the molten pool and the residual protective gas cannot escape in time, pores will form in the cladding layer. In addition, the poor morphology of the cladding layer is also a problem that needs to be solved. Poor morphology may manifest as uneven surface, poor bonding between the cladding layer and the substrate, etc., which will also affect the performance and service life of the cladding layer.
[0005] To address this problem, the present invention is implemented through the following contents. Summary of the invention
[0006] The purpose of the present invention is to provide a friction stir process for improving the performance of laser metal deposited TC4 alloy, which mainly solves the problem that in the prior art titanium alloy processing, large residual stress will be generated during the rapid heating and cooling of the substrate and the cladding material by a high-power laser beam, resulting in easy cracking and pore formation of the cladding layer.
[0007] To achieve the purpose, the present invention is implemented by the following technical scheme: a friction stir process for improving the performance of laser metal deposition TC4 alloy, mainly comprising the following specific steps: Step 1, putting TC4 titanium alloy powder into a beaker and placing it in a drying oven for drying to obtain dried powder; Step 2, grinding and cleaning the TC4 forged substrate to serve as a substrate for laser metal deposition; Step 3, the dried powder is deposited onto the treated substrate by synchronous powder feeding laser metal deposition to obtain 3 mm TC4 titanium alloy; Step 4: placing the deposited TC4 titanium alloy on a friction stir processing table and performing friction stir processing to obtain a stirred TC4 titanium alloy.
[0008] Optionally, the laser metal deposition process parameters are: laser power of 1400 W, scanning speed of 540 mm / min, spot diameter of 6 mm, powder feeding amount of 6 g / min, defocusing amount of 36 mm, and overlap rate of 45%.
[0009] Optionally, the stir friction processing parameter range is a travel speed of 50-130mm / min, a rotation speed of 450-850r / min, a stirring head shoulder pressure of 0.1±0.5mm, a stirring head stirring needle length of 2mm, a stirring needle shape of a truncated cone, a small truncated cone diameter at the end of which is 1±0.2mm, and a large truncated cone diameter at the root of which is 4±0.2mm.
[0010] The present invention can effectively eliminate defects in the organization by performing friction stir processing on the deposited TC4 titanium alloy, regulate the organizational morphology of the friction stir processing area, and achieve the purpose of grain refinement. During the friction stir processing, the stirring head rotates and moves inside the workpiece, and friction heat is generated at the same time. This friction heat can evenly heat the workpiece, reduce the temperature gradient between the welding or processing area and the surrounding materials, thereby reducing the thermal stress caused by the temperature difference. At the same time, the stirring process causes the material to undergo severe plastic deformation, mixing, and crushing, thereby achieving the densification, homogenization and refinement of the microstructure and eliminating the original defects (bubbles and cracks). Further, by controlling the parameters of the stirring head (rotation speed, travel speed), the heat input and heat distribution are better controlled, so that the residual stress and defects are effectively reduced or even eliminated after the processing is completed. The process of the present invention can efficiently and quickly process a grain-refined titanium alloy organization, and can improve the mechanical properties of the titanium alloy; the processing is green and environmentally friendly, low cost, easy to implement, and has good effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] By reading the detailed description below with reference to the accompanying drawings, the above and other objects, features and advantages of the exemplary embodiments of the present invention will become readily understood. In the accompanying drawings, several embodiments of the present invention are shown in an exemplary and non-limiting manner, and the same or corresponding reference numerals represent the same or corresponding parts, wherein: Figure 1 is a process flow chart of the method of the present invention; Figure 2 This is a SEM image of the microstructure of the deposited TC4 titanium alloy in an embodiment of the present invention; Figure 3 TC4 titanium alloy microstructure diagram with different stirring parameters in the embodiment of the present invention; Figure 4 The friction coefficient of TC4 titanium alloy with different stirring parameters in the embodiment of the present invention varies with time; Figure 5: This is an XRD comparison diagram of the optimal stirring state and the deposition state in the embodiment of the present invention; Figure 6 is a curve diagram showing the change of the friction coefficient (COF) over time in the optimal stirring state and the deposition state in an embodiment of the present invention; Figure 7 A comparison diagram of the wear rate and wear amount in the deposition state and the stirring state in the embodiment of the present invention; Figure 8 A comparison diagram of the Vickers hardness value changes in the deposition state and the stirring state in the embodiment of the present invention; Fig. 9 1 is a comparison diagram of electrochemical corrosion polarization curves in the deposition state and the stirring state in the embodiment of the present invention. DETAILED DESCRIPTION
[0012] The exemplary embodiments of the present disclosure will be described in more detail below with reference to the accompanying drawings. Although the exemplary embodiments of the present disclosure are shown in the accompanying drawings, it should be understood that the present disclosure can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present disclosure and to fully convey the scope of the present disclosure to those skilled in the art. If not specifically stated, the technical means used in the embodiments are conventional means well known to those skilled in the art.
[0013] In a first aspect, a friction stir process for improving the performance of laser metal deposited TC4 alloy comprises the following steps: Step 1, putting TC4 titanium alloy powder into a beaker and placing it in a drying oven for drying to obtain dried powder; Step 2, grinding and cleaning the TC4 forged substrate to serve as a substrate for laser metal deposition; Step 3, the dried powder is deposited onto the treated substrate by synchronous powder feeding laser metal deposition to obtain 3 mm TC4 titanium alloy; The dried powder was printed onto the treated forged TC4 substrate by laser metal deposition equipment. The laser power was 1400W, the scanning speed was 540mm / min, the powder feeding speed was 6g / min, the spot diameter was 6mm, the defocus was 36mm, the overlap rate was 45%, and it was carried out under oxygen-rich conditions. Finally, a 3mm thick deposited TC4 titanium alloy was obtained. Step 4, placing the deposited TC4 titanium alloy on a friction stir processing table, performing friction stir processing, and obtaining a stirred TC4 titanium alloy; Among them, the stirring needle length of the stirring head is set to 2mm, the shape of the stirring needle is truncated cone, the diameter of the small cone at the end is 1±0.2mm, the diameter of the large cone at the root is 4±0.2mm, the stirring speed is 50-130mm / min, the rotation speed is 450-850r / min, and the downward pressure of the stirring head shoulder is 0.1±0.5mm.
[0014] Then, stir friction processing was carried out based on different parameter combinations to obtain stirred TC4 titanium alloy. The microstructure observation and wear resistance test of the stirred TC4 alloy under different parameter combinations were carried out to obtain the influence of stirring parameters on the deposited TC4 titanium alloy and the optimal stirring parameters. The stirred TC4 titanium alloy obtained according to the optimal stirring parameters was compared with the deposited TC4 titanium alloy to obtain the enhanced performance parameters of the stirred TC4 titanium alloy. Example
[0015] The substrate used in the experiment in this test example is TC4 forging substrate, and the powder is TC4 spherical powder with a diameter of 50-150 μm; Powder drying: put the mixed powder into a beaker and dry it in a vacuum oven at 150°C for 12 hours; Substrate pretreatment: sandblasting the substrate surface for decontamination and then cleaning the surface with alcohol; Laser metal deposition: The RC-HSLC-6000 ultra-high-speed cladding equipment of Nanjing Zhongke Yuchen Co., Ltd. in China was selected, which was equipped with the RFL-C6000 laser device (maximum power 6000W) of Wuhan Raycus Fiber Laser Technology Co., Ltd. The nozzle uses coaxial four-way powder feeding, and the powder feeding gas and protective gas are both argon. The laser cladding process parameters are: laser power of 1400 W, scanning speed of 540 mm / min, spot diameter of 6 mm, powder feeding amount of 6g / min, defocusing amount of 36mm, and overlap rate of 45%.
[0016] Friction stir processing: Aerospace Technology Beijing Sai Foster Technology Co., Ltd. produces static gantry friction stir welding equipment, the equipment model is FSW-LM-AM20-2D, using tungsten rhenium alloy stirring head for stirring processing, the friction stir processing parameter range is travel speed 50-130mm / min, rotation speed 450-850r / min, stirring head shoulder pressure 0.1±0.5mm, stirring head stirring needle length 2mm, stirring needle shape is truncated cone, the end of the small cone diameter is 1±0.2mm, the root of the large cone diameter is 4±0.2mm, according to Table 1 to carry out stirring processing test, and then observe the wear resistance and microstructure of each group of data, and finally combine Figure 2 and Figure 3Number 3 was determined to be the optimal parameter. The microstructure and mechanical properties of stirred TC4 and deposited TC4 under the optimal parameters were observed and compared. Number Rotation speed Travel speed 1 450 90 2 650 90 3 850 90 4 850 50 5 850 130
[0017] Microstructure observation and mechanical properties test: Phase composition and microstructure: The prepared TC4 titanium alloy was cut into specimens of different sizes by wire cutting. The cut specimens were inlaid and then ground and polished. The inlaid specimens were corroded by etching solution for 60 seconds, and the surface was immediately cleaned with ethanol. The microstructure and element distribution of the coating were analyzed by Olympus BX53M optical microscope (OM), Olympus DSX1000 super depth of field microscope, CIQTEKSEM3100 scanning electron microscope (SEM) and Oxford Xplore15 energy dispersive spectrometer (EDS); the phase composition of the coating was analyzed by Rigaku UltimaIV X-ray diffractometer (XRD).
[0018] Microhardness: Use HVS-1000 Vickers microhardness tester to test the hardness of the coating along the vertical direction of the coating, apply a load of 1kg, and hold the load for 15s. Each test point is 200μm apart in the vertical direction of the coating, and 5 points at the same height are measured and the average value is taken as the hardness value of the point.
[0019] Friction and wear: The friction and wear test uses a reciprocating friction and wear machine. Before the test, the surface of the specimen is polished with sandpaper, then placed in an ultrasonic cleaner and cleaned with alcohol, and finally cleaned with deionized water and blown dry. The weight of the specimen is measured using an electronic balance. Each specimen is measured 5 times, and the average value is taken as the specimen weight. The test was carried out at room temperature and dry friction conditions. Friction and wear test conditions: load of 500 N, sliding speed of 30 mm / s, amplitude of 4 mm, frequency of 1 Hz, and test time of 30 min. After the test, the weight of the specimen after friction and wear was cleaned with an ultrasonic cleaner and measured, and the wear amount was calculated; the wear mark morphology and depth were observed with an ultra-depth of field microscope, and the surface wear morphology was analyzed with a scanning electron microscope (SEM).
[0020] Electrochemical corrosion: The electrochemical corrosion test was conducted using an electrochemical workstation. Before the test, the surface of the specimen was sanded and then polished to ensure that there were no obvious scratches on the coating surface. The non-test surface of the specimen was sealed with epoxy resin, leaving a 0.36 cm 2The test area is 3.5 wt% NaCl solution. The polarization curve of the specimen is measured, and the corrosion potential Ecorr and corrosion current density Icorr electrochemical parameters of each specimen are compared according to the polarization curve. After the polarization curve test is completed, the corroded surface of the specimen is cleaned with an ultrasonic cleaner, and the morphology after corrosion is observed using a scanning electron microscope (SEM).
[0021] Figure 2 The microstructure of the deposited TC4 titanium alloy is an equiaxed structure with a basketweave structure inside.
[0022] Figure 3 Indicates the microstructure morphology of the stirred state under different stirring parameters. Figure 3 It can be seen that after the third group of experiments, while the deposited equiaxed crystals were refined, their internal structure also became a layered structure with uniform tissue distribution. Although the first and fourth groups also refined the grains, the tissue formation was not as complete as the third group. The second and fifth groups became dual-state structures.
[0023] Figure 4 It shows the wear resistance under different stirring parameters. It can be seen that the friction coefficient of the third group is lower, so the rotating test parameters of the third group are the optimal parameters.
[0024] Figure 5 The XRD patterns of the deposited state and the optimal stirring state are shown. Figure 5 It can be seen that the stirred state shows the same phase characteristics as the deposited state, only the ratio of α phase and β phase in the alloy is changed, but the crystal plane strength is enhanced, which further confirms the process of grain refinement. During the friction stir processing, the content of β phase increases significantly due to the increase in temperature and reaching the β phase transition temperature.
[0025] Combination Figure 6 As shown in the figure, the curves of the change of the friction coefficient (COF) of the stirred state and the deposited state with time, the wear process of the parts can be divided into three stages: running-in stage, stable wear stage and severe wear stage. It can be found in the figure that the friction coefficient of the parts shows large fluctuations before 400 seconds for the LMD sample and before 150 seconds for the FSP sample. This stage is the running-in stage; after that, the friction coefficient gradually stabilizes and enters the stable wear stage. It is worth noting that during the stable wear stage of the sample, there is a part of the time when the friction coefficient fluctuates greatly. This is mainly because the wear debris generated during the wear process partially stays on the wear surface, resulting in greater jitter. After 1550 seconds, the fluctuation of the friction coefficient of the two samples began to show an increasing trend, which indicates that the parts have entered the severe wear stage. The friction coefficients of TC4 titanium alloys in the deposited and stirred states are 0.47 and 0.41, respectively. As Figure 7As shown, the wear rate and wear amount of the deposition state and the stirring state, it was finally concluded that the wear resistance was enhanced after stirring.
[0026] Figure 8 The graphs showing the changes in Vickers hardness values in the deposition state and the stirring state show that the thermomechanical effects generated during the stirring process caused the original coarse equiaxed grains to become finer, and the microstructure after the stirring was completed changed from the original basket structure to a layered structure, resulting in an increase in hardness.
[0027] Depend on Fig. 9 It can be seen that the corrosion potential Ecorr of the deposited sample is -1.004 V, the corrosion current density Icorr is -3.38×10-4 A·cm-2, the passive current density Ipass is 2.56×10-4 A·cm-2, and the breakdown potential Eb is 0.587V; the corrosion potential of the stirred TC4 alloy is basically unchanged, the corrosion current density Icorr decreases to -3.06×10-4 A·cm-2, the passive current density Ipass decreases to 1.04×10-4 A·cm-2, and the breakdown potential Eb does not change significantly. The passive current density is an important parameter for measuring passivation materials. A small passive current density indicates that the material has strong corrosion resistance. Therefore, the corrosion resistance of the stirred sample is better than that of the deposited state.
[0028] In summary, the present invention can effectively eliminate defects in the organization by performing stir friction processing on the deposited TC4 titanium alloy, regulate the organizational morphology of the stir friction processing area, and achieve the purpose of grain refinement. During the stir friction processing, the stirring head rotates and moves inside the workpiece, and friction heat is generated at the same time. This friction heat can evenly heat the workpiece, reduce the temperature gradient between the welding or processing area and the surrounding materials, thereby reducing the thermal stress caused by the temperature difference. At the same time, the stirring process causes the material to undergo severe plastic deformation, mixing, and crushing, thereby achieving the densification, homogenization and refinement of the microstructure and eliminating the original defects (bubbles and cracks). Further, by controlling the parameters of the stirring head (rotation speed, travel speed), the heat input and heat distribution are better controlled, so that the residual stress and defects are effectively reduced or even eliminated after the processing is completed. The process of the present invention can efficiently and quickly process a grain-refined titanium alloy organization, and can improve the mechanical properties of the titanium alloy; the processing is green and environmentally friendly, low cost, easy to implement, and has good effects.
[0029] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A friction stir process for improving the performance of laser metal deposited TC4 alloy, characterized in that: The following steps are involved: Step 1, putting TC4 titanium alloy powder into a beaker, placing it in a drying oven for drying, and obtaining dried powder; Step 2: Grind and clean the TC4 forged substrate to serve as a substrate for laser metal deposition; Step 3, the dried powder is deposited onto the treated substrate by synchronous powder feeding laser metal deposition to obtain a TC4 titanium alloy with a coating thickness of 3 mm; Step 4: placing the deposited TC4 titanium alloy on a friction stir processing table and performing friction stir processing to obtain a stirred TC4 titanium alloy.
2. The friction stir process for improving the performance of laser metal deposited TC4 alloy according to claim 1, characterized in that: The step 3 comprises: The dry powder was printed onto the treated forged TC4 substrate by laser metal deposition equipment. The laser power was 1400W, the scanning speed was 540mm / min, the powder feeding speed was 6g / min, and the spot diameter was 6mm. The defocus amount was 36mm, the overlap rate was 45%, and it was carried out under oxygen-rich conditions, and finally a 3mm thick deposited TC4 titanium alloy was obtained.
3. The friction stir process for improving the performance of laser metal deposited TC4 alloy according to claim 1, characterized in that: In step 4, the stirring speed is 50-130 mm / min, the rotation speed is 450-850 r / min, and the downward pressure of the stirring head shoulder is 0.1±0.5 mm.
4. The friction stir process for improving the performance of laser metal deposited TC4 alloy according to claim 1, characterized in that: In step 4, the stirring needle of the stirring head is 2 mm long and truncated cone-shaped, with a small cone at the end having a diameter of 1±0.2 mm and a large cone at the root having a diameter of 4±0.2 mm.
5. The friction stir process for improving the performance of laser metal deposited TC4 alloy according to claim 1, characterized in that: In step 4, stir friction processing is performed based on different parameter combinations to obtain a stirred TC4 titanium alloy, and microstructure observation and wear resistance testing are performed on the stirred TC4 alloy under different parameter combinations to obtain the influence of the stirring parameters on the deposited TC4 titanium alloy and the optimal stirring parameters.
6. The friction stir process for improving the performance of laser metal deposited TC4 alloy according to claim 5, characterized in that: The stirred TC4 titanium alloy obtained according to the optimal stirring parameters is compared with the deposited TC4 titanium alloy to obtain the enhanced performance parameters of the stirred TC4 titanium alloy.
Citation Information
Patent Citations
Laser cladding-stirring friction composite surface modification method
CN108385113A