Steel fastener, machining method thereof, part and automobile

By setting galvanized layer, passivation layer and isolation layer on the surface of steel fasteners, the corrosion problem of steel fasteners at the connection of alloy components is solved, the corrosion resistance and fastening force are improved, and the vehicle is ensured. reliability.

CN118957581APending Publication Date: 2024-11-15DONGFENG COMML VEHICLE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411031188.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing steel fasteners are prone to corrosion at the connection between alloy components and steel fasteners, affecting the reliability of the vehicle.

Method used

The steel fastener is equipped with a galvanized layer, a passivation layer and an isolation layer. The passivation layer is composed of chromium trichloride, oxalic acid, sodium nitrate cobalt sulfate and citric acid. The isolation layer is composed of trimethoxymethylsilane, poly The combination of tetrafluoroethylene, silicone leveling agent and aluminum powder is composed of which improves the anti-rust performance and friction coefficient stability through the combination of these layers, and avoids contact corrosion.

Benefits of technology

It effectively improves the corrosion resistance and fastening force of steel fasteners, ensures stable connection with aluminum alloy or stainless steel components, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004969961290000121
    Figure BDA0004969961290000121
  • Figure BDA0004969961290000131
    Figure BDA0004969961290000131
Patent Text Reader

Abstract

The invention discloses a steel fastener, a machining method of the steel fastener, a part and an automobile, and relates to the technical field of vehicles. Comprising a steel fastener body, and a zinc coating, a passivation layer and an isolation layer which are sequentially arranged on the surface of the steel fastener body from inside to outside, wherein the passivation layer is made of chromium trichloride, oxalic acid, sodium nitrate, cobaltous sulfate and citric acid; the isolating layer is made of trimethoxymethylsilane, polytetrafluoroethylene, an organic silicon flatting agent and aluminum powder. And the zinc coating and the passivation layer are bottom layers, so that the anti-rust performance and easy adhesiveness of the steel fastener can be improved. The passivation layer is coated with the isolation layer, the silver isolation layer contains friction coefficient stable components and has excellent adhesive force and friction coefficient stability, and when the fastener is tightened on an aluminum alloy or stainless steel component for fastening, the isolation layer isolates the steel fastener from the aluminum alloy or stainless steel component, so that contact corrosion is avoided, and the service life of the fastener is prolonged. And meanwhile, the fastening force is ensured by the stable friction coefficient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of automobile technology, and in particular to a steel fastener and a processing method thereof, a part and an automobile. Background Art

[0002] With the development of economy, various types of vehicles have entered people's lives. In order to meet the different load-bearing requirements of different components, components with dissimilar metal contacts often appear on vehicles, usually the connection between alloy components and steel fasteners.

[0003] As the use time increases and the use environment changes, corrosion of steel fasteners will occur at the connection points between alloy components and steel fasteners, thereby affecting the reliability of the vehicle. Summary of the invention

[0004] The present application provides a steel fastener and a processing method thereof, a part and an automobile to solve the corrosion problem of existing steel fasteners.

[0005] In a first aspect, the present application provides a steel fastener, comprising a steel fastener body and a galvanized layer, a passivation layer and an isolation layer sequentially arranged on the surface of the steel fastener body from the inside to the outside, wherein:

[0006] The material of the passivation layer includes chromium trichloride, oxalic acid, sodium nitrate, cobalt sulfate and citric acid;

[0007] The materials of the isolation layer include trimethoxymethylsilane, polytetrafluoroethylene, organic silicon leveling agent and aluminum powder.

[0008] The present application sets a galvanized layer, a passivation layer and an isolation layer on the surface of the steel fastener. The galvanized layer and the passivation layer are the bottom layer, which can improve the rust resistance and adhesion of the steel fastener. The isolation layer is coated on the passivation layer. The silver isolation layer contains friction coefficient stabilizing components and has excellent adhesion and friction coefficient stability. When the fastener is tightened on the aluminum alloy or stainless steel part, the isolation layer isolates the steel fastener from the aluminum alloy or stainless steel part, thereby avoiding contact corrosion. At the same time, the stable friction coefficient ensures the fastening force.

[0009] Among them, in the passivation layer, chromium trichloride and oxalic acid will undergo a complex reaction to generate chromium oxalate, which is the main component of the passivation film. Sodium nitrate plays a role in accelerating the passivation reaction and accelerating the film formation, so that the passivation layer can be formed. Cobalt sulfate makes the passivation layer have good corrosion resistance. The complexation rate is increased by complexing chromium trichloride with oxalic acid, thereby increasing the thickness of the passivation film. The passivation reacts quickly by catalysis of sodium nitrate. The acidity of the passivation reaction is reduced by citric acid, so that the passivation film is dissolved while the passivation agent reacts quickly to generate a thick film. Under this dynamic balance, a loose passivation film structure is finally generated.

[0010] In the isolation layer, trimethoxymethylsilane is the main film-forming agent and the main component of the isolation layer formed on the surface of the part. Its main function is to ensure a certain thickness to achieve isolation and rust prevention effects. At the same time, as a component that stabilizes the friction coefficient, it provides a carrier for other friction coefficient stabilizing components. Polytetrafluoroethylene (PTFE) is a friction coefficient regulating component. The friction coefficient of trimethoxymethylsilane is high, and the friction coefficient of polytetrafluoroethylene (PTFE) is low. Through the adjustment of the two components, the friction coefficient of the isolation layer formed on the surface of the part can be kept stable. The function of the silicone leveling agent is to ensure that the thickness of the isolation layer is uniform and the appearance is smooth. The main function of the aluminum paste is to adjust the appearance color of the isolation layer, and at the same time, it plays a role in adjusting the electrode potential of the isolation layer. Further reduce the contact corrosion of steel fasteners.

[0011] The passivating agent forms a passivation film on the galvanized layer. The passivation film can increase the rust resistance of the galvanized layer, that is, improve the corrosion resistance of the steel fasteners. In the present application, due to the presence of citric acid, the dense passivation film is dissolved into a loose non-dense film layer, thereby improving the adhesion of the isolation agent on the passivation film. The formed isolation layer is mutually infiltrated and compounded with the galvanized layer and the passivation layer, rather than a simply superimposed film layer, which further improves the isolation and rust prevention effects.

[0012] In some embodiments, in the material of the passivation layer, the mass ratio of chromium trichloride, oxalic acid, sodium nitrate cobalt sulfate and citric acid is (25-35): (50-60): (3-5): (8-12): (1-3). In the material of the passivation layer, the mass ratio of chromium trichloride, oxalic acid, sodium nitrate cobalt sulfate and citric acid is within this range, which can form a loose and porous passivation layer. The appropriate proportion of oxalic acid can dissolve the passivation layer at an appropriate rate, so that the pores of the passivation layer are maintained at an appropriate size, thereby improving the adhesion between the passivation layer and the isolation layer.

[0013] In some embodiments, in the material of the isolation layer, the mass ratio of trimethoxymethylsilane, polytetrafluoroethylene, silicone leveling agent and aluminum powder is (45-50): (3-8): (15-20): (4-6). The mass ratio of trimethoxymethylsilane, polytetrafluoroethylene, silicone leveling agent and aluminum powder in the isolation layer is within this range, which can further stabilize the friction coefficient of the isolation layer within a suitable range, and at the same time, the color of the isolation layer is closer to that of the alloy part, reducing color difference.

[0014] In some embodiments, the thickness of the galvanized layer is 10-12 μm. When the thickness of the galvanized layer is within this range, the corrosion resistance of the steel fastener can be further improved; and / or,

[0015] The thickness of the passivation layer is 2 to 3 μm. When the thickness of the passivation layer is within this range, the adhesion between the isolation layer and the passivation layer can be improved; and / or,

[0016] The thickness of the isolation layer is 4-6 μm. When the thickness of the isolation layer is within this range, the fastener will not be unable to be screwed in due to the coating being too thick when being tightened, and the coating will not be damaged and lose its isolation function after the fastener is tightened.

[0017] In a second aspect, the present application proposes a method for processing a steel fastener, comprising the following steps:

[0018] The steel fastener body is subjected to galvanizing treatment to obtain a steel fastener body containing a galvanized layer;

[0019] preparing the material of the passivation layer into a passivation layer slurry;

[0020] Dipping the steel fastener body containing the galvanized layer into the passivation layer slurry to form the passivation layer, thereby obtaining the steel fastener body containing the passivation layer;

[0021] preparing the material of the isolation layer into isolation layer slurry;

[0022] The steel fastener body containing the passivation layer is immersed in the isolation layer slurry to form the isolation layer, thereby obtaining the steel fastener.

[0023] The preparation method of the passivation layer slurry can be to fully complex chromium trichloride with oxalic acid and then fully mix it with other ingredients.

[0024] The solvent in the isolation layer slurry can be CAC to ensure the dispersion and stability of the ingredients in the formula. It evaporates during the baking process and has no effect on the performance of the isolation layer finally formed on the surface of the part.

[0025] The complexation conditions of chromium trichloride and oxalic acid can be 100-150° C., and the complexation time can be 1-3 hours.

[0026] The passivation agent slurry forms a passivation film on the galvanized layer. The passivation film can increase the rust resistance of the galvanized layer, that is, improve the corrosion resistance of the steel fasteners. In the present application, due to the presence of citric acid, the dense passivation film is dissolved into a loose non-dense film layer, thereby improving the adhesion of the isolation agent on the passivation film. The formed isolation layer is mutually infiltrated and compounded with the galvanized layer and the passivation layer, rather than a simply superimposed film layer, which further improves the isolation and rust prevention effects.

[0027] In some embodiments, the steel fastener body containing the galvanized layer is immersed in a passivation layer slurry to form a passivation layer, and the steel fastener body containing the passivation layer is obtained:

[0028] The immersion time is 1 to 2.5 minutes. When the immersion time is within this range, it can help to form a loose passivation layer, improve the wear resistance of the passivation layer and the adhesion to the isolation layer.

[0029] In some embodiments, the steel fastener body containing the passivation layer is immersed in the isolation layer slurry to form the isolation layer, and the steel fastener comprises:

[0030] Dipping the steel fastener body containing the passivation layer into the isolation layer slurry to form a first wet isolation layer, thereby obtaining the steel fastener body containing the first wet isolation layer;

[0031] Centrifuging and drying the steel fastener body containing the first wet isolation layer to form a first dry isolation layer, thereby obtaining a steel fastener body containing the first dry isolation layer;

[0032] Dipping the steel fastener body containing the first dry isolation layer into the isolation layer slurry to form a second wet isolation layer, thereby obtaining the steel fastener body containing the second wet isolation layer;

[0033] The steel fastener body containing the second wet isolation layer is centrifuged and dried to form a second dry isolation layer, thereby obtaining the steel fastener body.

[0034] Through two film-forming and two drying processes, the bottom exposure caused by scratches and bumps can be reduced, while ensuring that the isolation layer reaches 4-6μm. In the isolation layer, trimethoxymethylsilane is the main film-forming agent and the main component of the isolation layer formed on the surface of the part. Its main function is to ensure a certain thickness to achieve isolation and rust prevention effects. At the same time, as a component that stabilizes the friction coefficient, it provides a carrier for other friction coefficient stabilizing components. Polytetrafluoroethylene (PTFE) is a friction coefficient regulating component. The friction coefficient of trimethoxymethylsilane is higher, while the friction coefficient of polytetrafluoroethylene (PTFE) is lower. Through the adjustment of the two components, the friction coefficient of the isolation layer formed on the surface of the part can be kept stable. The function of the silicone leveling agent is to ensure that the thickness of the isolation layer is uniform and the appearance is smooth. The main function of the aluminum paste is to adjust the appearance color of the isolation layer and to adjust the electrode potential of the isolation layer. Further reduce the contact corrosion of steel fasteners.

[0035] In some embodiments, the immersion time is 0.5 to 2 minutes; and / or,

[0036] The centrifugal speed is 200-400 r / min; and / or,

[0037] The centrifugation time is 0.5 to 2 minutes; and / or,

[0038] The baking temperature is 150-200°C; and / or,

[0039] The baking time is 15 to 45 minutes.

[0040] Under the above centrifugal rate, centrifugal time, baking temperature and baking time, the isolation layer can have a uniform appearance and a consistent thickness, which can stably reach 4-6μm. At the same time, the isolation layer can have good adhesion and reduce damage to the passivation layer.

[0041] In a third aspect, the present application provides a part, including the steel fastener of the first aspect, or a steel fastener made by the processing method of the steel fastener of the second aspect. The part includes but is not limited to a stainless steel hoop for automobiles, an EGR guard plate, an aluminum alloy workbench, an aluminum wheel, an aluminum gearbox bottom shell, etc.

[0042] In a fourth aspect, the present application provides a car comprising the parts of the third aspect. DETAILED DESCRIPTION

[0043] In order to make the purpose, technical solution and advantages of the present application clearer, the technical solution of the present application will be clearly and completely described below in combination with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.

[0044] With the development of economy, various types of vehicles have entered people's lives. In order to meet the different load-bearing requirements of different components, components with dissimilar metal contacts often appear on vehicles, usually the connection between alloy components and steel fasteners.

[0045] As the use time increases and the use environment changes, corrosion of steel fasteners will occur at the connection points between alloy components and steel fasteners, thereby affecting the reliability of the vehicle.

[0046] The current solutions to this problem mainly include: 1) using fasteners made of the same material as the connected parts; 2) using zinc-nickel alloy fasteners; 3) coating the surfaces of the connected parts with organic isolation coatings such as paint;

[0047] 4) Install rubber gaskets between fasteners and connected parts. However, there are many problems with the above method. When fasteners are made of the same material as the connected parts, the strength performance of aluminum fasteners and stainless steel fasteners can only reach 8.8. For some parts with large tightening torque, 10.9 is required, and the strength performance is not currently achieved. For fasteners made of zinc-nickel alloy, the nickel content in the zinc-nickel alloy layer is 8-12%, and there is still a large electrode potential difference with aluminum or stainless steel. The zinc-nickel alloy can only be more corrosion-resistant than galvanizing and Dacromet, but it cannot meet the corrosion resistance requirements of vehicles. Paint the surface of the connected parts with organic isolation coatings such as paint. Aluminum alloy and stainless steel parts are often required to maintain their original color and have a large area, and the cost of coating is very high. Install rubber gaskets between fasteners and connected parts. In parts where large tightening torque is required, the rubber gaskets will affect the axial tightening force and cause loosening.

[0048] In view of this, the present application provides a steel fastener and a processing method thereof, a part and an automobile to solve the corrosion problem of existing steel fasteners.

[0049] In a first aspect, the present application provides a steel fastener, comprising a steel fastener body and a galvanized layer, a passivation layer and an isolation layer sequentially arranged on the surface of the steel fastener body from the inside to the outside, wherein:

[0050] The material of the passivation layer includes chromium trichloride, oxalic acid, sodium nitrate, cobalt sulfate and citric acid;

[0051] The materials of the isolation layer include trimethoxymethylsilane, polytetrafluoroethylene, organic silicon leveling agent and aluminum powder.

[0052] The present application sets a galvanized layer, a passivation layer and an isolation layer on the surface of the steel fastener. The galvanized layer and the passivation layer are the bottom layer, which can improve the rust resistance and adhesion of the steel fastener. The isolation layer is coated on the passivation layer. The silver isolation layer contains friction coefficient stabilizing components and has excellent adhesion and friction coefficient stability. When the fastener is tightened on the aluminum alloy or stainless steel part, the isolation layer isolates the steel fastener from the aluminum alloy or stainless steel part, thereby avoiding contact corrosion. At the same time, the stable friction coefficient ensures the fastening force.

[0053] Among them, in the passivation layer, chromium trichloride and oxalic acid will undergo a complex reaction to generate chromium oxalate, which is the main component of the passivation film. Sodium nitrate plays a role in accelerating the passivation reaction and accelerating the film formation, so that the passivation layer can be formed. Cobalt sulfate makes the passivation layer have good corrosion resistance. The complexation rate is increased by complexing chromium trichloride with oxalic acid, thereby increasing the thickness of the passivation film. The passivation reacts quickly by catalysis of sodium nitrate. The acidity of the passivation reaction is reduced by citric acid, so that the passivation film is dissolved while the passivation agent reacts quickly to generate a thick film. Under this dynamic balance, a loose passivation film structure is finally generated.

[0054] In the isolation layer, trimethoxymethylsilane is the main film-forming agent and the main component of the isolation layer formed on the surface of the part. Its main function is to ensure a certain thickness to achieve isolation and rust prevention effects. At the same time, as a component that stabilizes the friction coefficient, it provides a carrier for other friction coefficient stabilizing components. Polytetrafluoroethylene (PTFE) is a friction coefficient regulating component. The friction coefficient of trimethoxymethylsilane is high, and the friction coefficient of polytetrafluoroethylene (PTFE) is low. Through the adjustment of the two components, the friction coefficient of the isolation layer formed on the surface of the part can be kept stable. The function of the silicone leveling agent is to ensure that the thickness of the isolation layer is uniform and the appearance is smooth. The main function of the aluminum paste is to adjust the appearance color of the isolation layer, and at the same time, it plays a role in adjusting the electrode potential of the isolation layer. Further reduce the contact corrosion of steel fasteners.

[0055] The passivating agent forms a passivation film on the galvanized layer. The passivation film can increase the rust resistance of the galvanized layer, that is, improve the corrosion resistance of the steel fasteners. In the present application, due to the presence of citric acid, the dense passivation film is dissolved into a loose non-dense film layer, thereby improving the adhesion of the isolation agent on the passivation film. The formed isolation layer is mutually infiltrated and compounded with the galvanized layer and the passivation layer, rather than a simply superimposed film layer, which further improves the isolation and rust prevention effects.

[0056] In combination with the first aspect, in some embodiments provided in the present application, in the material of the passivation layer, the mass ratio of chromium trichloride, oxalic acid, sodium nitrate cobalt sulfate and citric acid is (25-35): (50-60): (3-5): (8-12): (1-3). In the material of the passivation layer, the mass ratio of chromium trichloride, oxalic acid, sodium nitrate cobalt sulfate and citric acid is within this range, which can form a loose and porous passivation layer. The appropriate proportion of oxalic acid can dissolve the passivation layer at an appropriate rate, so that the pores of the passivation layer are maintained at an appropriate size, thereby improving the adhesion between the passivation layer and the isolation layer.

[0057] In combination with the first aspect, in some embodiments provided in the present application, in the material of the isolation layer, the mass ratio of trimethoxymethylsilane, polytetrafluoroethylene, silicone leveling agent and aluminum powder is (45-50): (3-8): (15-20): (4-6). The mass ratio of trimethoxymethylsilane, polytetrafluoroethylene, silicone leveling agent and aluminum powder in the isolation layer is within this range, which can further stabilize the friction coefficient of the isolation layer within a suitable range, and at the same time, the color of the isolation layer is closer to that of the alloy part, reducing color difference.

[0058] In combination with the first aspect, in some embodiments provided in the present application, the thickness of the galvanized layer is 10 to 12 μm. When the thickness of the galvanized layer is within this range, the corrosion resistance of the steel fasteners can be further improved.

[0059] In combination with the first aspect, in some embodiments provided in the present application, the thickness of the passivation layer is 2 to 3 μm. When the thickness of the passivation layer is within this range, the adhesion between the isolation layer and the passivation layer can be improved.

[0060] In combination with the first aspect, in some embodiments provided in the present application, the thickness of the isolation layer is 4 to 6 μm. When the thickness of the isolation layer is within this range, the fastener will not be unable to be screwed in due to the coating being too thick, and the coating will not be damaged and lose its isolation function after the fastener is tightened.

[0061] In a second aspect, the present application proposes a method for processing a steel fastener, comprising the following steps:

[0062] The steel fastener body is subjected to galvanizing treatment to obtain a steel fastener body containing a galvanized layer;

[0063] preparing the material of the passivation layer into a passivation layer slurry;

[0064] Dipping the steel fastener body containing the galvanized layer into the passivation layer slurry to form the passivation layer, thereby obtaining the steel fastener body containing the passivation layer;

[0065] preparing the material of the isolation layer into isolation layer slurry;

[0066] The steel fastener body containing the passivation layer is immersed in the isolation layer slurry to form the isolation layer, thereby obtaining the steel fastener.

[0067] The preparation method of the passivation layer slurry can be to fully complex chromium trichloride with oxalic acid and then fully mix it with other ingredients.

[0068] The solvent in the isolation layer slurry can be CAC to ensure the dispersion and stability of the ingredients in the formula. It evaporates during the baking process and has no effect on the performance of the isolation layer finally formed on the surface of the part.

[0069] The complexation conditions of chromium trichloride and oxalic acid can be 100-150° C., and the complexation time can be 1-3 hours.

[0070] The passivation agent slurry forms a passivation film on the galvanized layer. The passivation film can increase the rust resistance of the galvanized layer, that is, improve the corrosion resistance of the steel fasteners. In the present application, due to the presence of citric acid, the dense passivation film is dissolved into a loose non-dense film layer, thereby improving the adhesion of the isolation agent on the passivation film. The formed isolation layer is mutually infiltrated and compounded with the galvanized layer and the passivation layer, rather than a simply superimposed film layer, which further improves the isolation and rust prevention effects.

[0071] In combination with the second aspect, in some embodiments provided in the present application, a steel fastener body containing a galvanized layer is immersed in a passivation layer slurry to form a passivation layer, thereby obtaining a steel fastener body containing a passivation layer: the immersion time is 1 to 2.5 minutes. The immersion time within this range can help form a loose passivation layer and improve the wear resistance of the passivation layer and the adhesion to the isolation layer.

[0072] In combination with the second aspect, in some embodiments provided in the present application, the steel fastener body containing the passivation layer is immersed in an isolation layer slurry to form an isolation layer, and the steel fastener comprises:

[0073] Dipping the steel fastener body containing the passivation layer into the isolation layer slurry to form a first wet isolation layer, thereby obtaining the steel fastener body containing the first wet isolation layer;

[0074] Centrifuging and drying the steel fastener body containing the first wet isolation layer to form a first dry isolation layer, thereby obtaining a steel fastener body containing the first dry isolation layer;

[0075] Dipping the steel fastener body containing the first dry isolation layer into the isolation layer slurry to form a second wet isolation layer, thereby obtaining the steel fastener body containing the second wet isolation layer;

[0076] The steel fastener body containing the second wet isolation layer is centrifuged and dried to form a second dry isolation layer, thereby obtaining the steel fastener body.

[0077] Through two film-forming and two drying processes, the exposed bottom caused by scratches and bumps during the first film-forming process can be compensated, while ensuring that the isolation layer reaches 4-6μm. In the isolation layer, trimethoxymethylsilane is the main film-forming agent and the main component of the isolation layer formed on the surface of the part. Its main function is to ensure a certain thickness to achieve isolation and rust prevention effects. At the same time, as a component that stabilizes the friction coefficient, it provides a carrier for other friction coefficient stabilizing components. Polytetrafluoroethylene (PTFE) is a friction coefficient regulating component. The friction coefficient of trimethoxymethylsilane is higher, while the friction coefficient of polytetrafluoroethylene (PTFE) is lower. Through the regulation of the two components, the friction coefficient of the isolation layer formed on the surface of the part can be kept in a stable state. The function of the silicone leveling agent is to ensure that the thickness of the isolation layer is uniform and the appearance is smooth. The main function of the aluminum paste is to adjust the appearance color of the isolation layer and to adjust the electrode potential of the isolation layer. Further reduce the contact corrosion of steel fasteners.

[0078] In combination with the second aspect, in some embodiments provided in the present application, the immersion time is 0.5 to 2 minutes.

[0079] In combination with the second aspect, in some embodiments provided in the present application, the centrifugal speed is 200-400 r / min.

[0080] In combination with the second aspect, in some embodiments provided in the present application, the centrifugation time is 0.5 to 2 minutes.

[0081] In combination with the second aspect, in some embodiments provided in the present application, the baking temperature is 150-200°C.

[0082] In combination with the second aspect, in some embodiments provided in the present application, the baking time is 15 to 45 minutes.

[0083] Under the above centrifugal rate, centrifugal time, baking temperature and baking time, the isolation layer can have a uniform appearance and a consistent thickness, which can stably reach 4-6μm. At the same time, the isolation layer can have good adhesion and reduce damage to the passivation layer.

[0084] In a third aspect, the present application provides a part, including the steel fastener of the first aspect, or a steel fastener made by the processing method of the steel fastener of the second aspect. The part includes but is not limited to a stainless steel hoop for automobiles, an EGR guard plate, an aluminum alloy workbench, an aluminum wheel, an aluminum gearbox bottom shell, etc. The part has all the beneficial effects of the steel fastener, and the present application will not repeat them one by one.

[0085] In a fourth aspect, the present application provides a car, comprising the parts of the third aspect. The car has all the beneficial effects of the steel fastener, which will not be described in detail in this application.

[0086] The technical solution provided in this application is described in detail below in conjunction with embodiments.

[0087] Example 1

[0088] Embodiment 1 of the present application provides a steel fastener and a processing method thereof.

[0089] 1) Steel fasteners

[0090] It comprises a steel fastener body and a 10 μm zinc plating layer, a 2 μm passivation layer and a 6 μm isolation layer which are sequentially arranged on the surface of the steel fastener body from the inside to the outside;

[0091] The material of the passivation layer includes chromium trichloride, oxalic acid, sodium nitrate, cobalt sulfate and citric acid, and the mass ratio thereof is 25:50:3:8:1;

[0092] The material of the isolation layer includes trimethoxymethylsilane, polytetrafluoroethylene, an organic silicon leveling agent and aluminum powder, and the mass ratio thereof is 45:7:18:5.

[0093] 2) A method for processing a steel fastener, comprising the following steps:

[0094] The steel fastener body is subjected to galvanizing treatment to obtain a steel fastener body containing a galvanized layer;

[0095] preparing the material of the passivation layer into a passivation layer slurry;

[0096] The steel fastener body containing the galvanized layer is immersed in the passivation layer slurry for 1 minute to form a passivation layer, thereby obtaining a steel fastener body containing the passivation layer;

[0097] The material of the isolation layer is prepared into an isolation layer slurry, wherein the solvent of the isolation layer is ethylene glycol ethyl ether acetate, and the mass ratio of ethylene glycol ethyl ether acetate to trimethoxymethylsilane is 45:25;

[0098] The steel fastener body containing the passivation layer is immersed in the isolation layer slurry with a viscosity of 13s (coating 4# cup) for 1 minute, then placed in a centrifuge with a centrifugal speed of 300r / min and a centrifugal time of 1 minute, and then baked in a mesh belt furnace with a baking temperature of 170°C and a baking time of 25 minutes, and naturally cooled; the above dipping process is repeated once to obtain a steel fastener.

[0099] Example 2

[0100] Embodiment 2 of the present application provides a steel fastener and a processing method thereof.

[0101] 1) Steel fasteners

[0102] It comprises a steel fastener body and a 12 μm zinc-plated layer, a 2.5 μm passivation layer and a 4 μm isolation layer which are sequentially arranged on the surface of the steel fastener body from the inside to the outside;

[0103] The material of the passivation layer includes chromium trichloride, oxalic acid, sodium nitrate, cobalt sulfate and citric acid, and the mass ratio thereof is 35:60:5:12:3;

[0104] The material of the isolation layer includes trimethoxymethylsilane, polytetrafluoroethylene, organic silicon leveling agent and aluminum powder, and the mass ratio thereof is 50:8:20:6.

[0105] 2) A method for processing a steel fastener, comprising the following steps:

[0106] The steel fastener body is subjected to galvanizing treatment to obtain a steel fastener body containing a galvanized layer;

[0107] preparing the material of the passivation layer into a passivation layer slurry;

[0108] The steel fastener body containing the galvanized layer is immersed in the passivation layer slurry for 2 minutes to form a passivation layer, thereby obtaining a steel fastener body containing the passivation layer;

[0109] The material of the isolation layer is prepared into an isolation layer slurry, wherein the solvent of the isolation layer is ethylene glycol ethyl ether acetate, and the mass ratio of ethylene glycol ethyl ether acetate to trimethoxymethylsilane is 50:35;

[0110] The steel fastener body containing the passivation layer is immersed in the isolation layer slurry with a viscosity of 13s (coating 4# cup) for 0.5min, then placed in a centrifuge with a centrifugal speed of 200r / min and a centrifugal time of 2min, and then baked in a mesh belt furnace with a baking temperature of 150°C and a baking time of 45min, and naturally cooled; the above dipping process is repeated once to obtain a steel fastener.

[0111] Example 3

[0112] Embodiment 3 of the present application provides a steel fastener and a processing method thereof.

[0113] 1) Steel fasteners

[0114] It comprises a steel fastener body and a 11 μm zinc-plated layer, a 3 μm passivation layer and a 5 μm isolation layer which are sequentially arranged on the surface of the steel fastener body from the inside to the outside;

[0115] The material of the passivation layer includes chromium trichloride, oxalic acid, sodium nitrate, cobalt sulfate and citric acid, and the mass ratio thereof is 30:55:4:10:2;

[0116] The material of the isolation layer includes trimethoxymethylsilane, polytetrafluoroethylene, an organic silicon leveling agent and aluminum powder, and the mass ratio thereof is 48:3:15:4.

[0117] 2) A method for processing a steel fastener, comprising the following steps:

[0118] The steel fastener body is subjected to galvanizing treatment to obtain a steel fastener body containing a galvanized layer;

[0119] preparing the material of the passivation layer into a passivation layer slurry;

[0120] The steel fastener body containing the galvanized layer is immersed in the passivation layer slurry for 2.5 minutes to form a passivation layer, thereby obtaining a steel fastener body containing the passivation layer;

[0121] The material of the isolation layer is prepared into an isolation layer slurry, wherein the solvent of the isolation layer is ethylene glycol ethyl ether acetate, and the mass ratio of ethylene glycol ethyl ether acetate to trimethoxymethylsilane is 48:30;

[0122] The steel fastener body containing the passivation layer is immersed in the isolation layer slurry with a viscosity of 13s (coating 4# cup) for 2 minutes, then placed in a centrifuge with a centrifugal speed of 400r / min and a centrifugal time of 0.5min, and then baked in a mesh belt furnace with a baking temperature of 200°C and a baking time of 15min, and naturally cooled; the above dipping process is repeated once to obtain a steel fastener.

[0123] Comparative Example 1

[0124] Comparative Example 1 of the present application provides a steel fastener and a processing method thereof. Comparative Example 1 is similar to Example 1, except that the passivation layer of Comparative Example 1 does not contain citric acid.

[0125] Comparative Example 2

[0126] Comparative Example 2 of the present application provides a steel fastener and a processing method thereof. Comparative Example 2 is similar to Example 1, except that the passivation layer material of Comparative Example 2 does not contain oxalic acid.

[0127] Comparative Example 3

[0128] Comparative Example 3 of the present application provides a steel fastener and a processing method thereof. Comparative Example 3 is similar to Example 1, except that Comparative Example 3 does not contain an isolation layer.

[0129] Comparative Example 4

[0130] Comparative Example 4 of the present application provides a steel fastener and a processing method thereof. Comparative Example 4 is similar to Example 1, except that the isolation layer of Comparative Example 4 does not contain polytetrafluoroethylene.

[0131] Comparative Example 5

[0132] Comparative Example 5 of the present application provides a steel fastener and a processing method thereof. Comparative Example 5 is similar to Example 1, except that the isolation layer of Comparative Example 5 does not contain trimethoxymethylsilane.

[0133] Comparative Example 6

[0134] Comparative Example 6 of the present application provides a steel fastener and a processing method thereof. Comparative Example 6 is similar to Example 1, except that the isolation layer of Comparative Example 6 does not contain aluminum powder.

[0135] The steel fasteners of Examples 1 to 3 and Comparative Examples 1 to 6 were tested for performance, and their appearance, neutral salt spray test duration when connected to aluminum alloy parts, neutral salt spray test duration when connected to stainless steel parts, SO2 gas corrosion test duration, friction coefficient and adhesion were tested, wherein the test methods are: neutral salt spray test (aluminum alloy) according to GB / T 10125; neutral salt spray test (stainless steel) according to GB / T 10125; SO2 gas corrosion test according to GB / T 9789; friction coefficient according to GB 3103.1; adhesion according to GB / T9286. The test results are shown in Table 1.

[0136] Table 1 Properties of steel fasteners of Examples 1 to 3 and Comparative Examples 1 to 6

[0137]

[0138]

[0139] As can be seen from Table 1, the steel fasteners of Examples 1 to 3 have a silvery white appearance, which is close to the color of aluminum alloy and stainless steel, and are resistant to a neutral salt spray test for 480 hours (testing standard GB / T 10125), a sulfur dioxide gas corrosion test for 96 hours (testing standard GB / T9789), a surface friction coefficient of 0.1-0.15 (GB / T 3098.1), and excellent comprehensive performance in resistance to salt corrosion and acid rain corrosion. The isolation layer has good adhesion and a stable friction coefficient. After the fastener is tightened, the steel fastener is isolated from the connected parts made of aluminum alloy or stainless steel, which prevents contact corrosion. At the same time, the stable friction coefficient can ensure the fastener torque of the fastener.

[0140] In Comparative Example 1, since the passivation layer does not contain citric acid, the thickness of the passivation layer becomes smaller and the passivation layer is incomplete, resulting in reduced adhesion of the isolation layer, and ultimately causing reduced overall performance.

[0141] In Comparative Example 2, since the passivation layer material does not contain oxalic acid, the thickness of the passivation layer becomes smaller and the passivation layer is incomplete, resulting in reduced adhesion of the isolation layer, and ultimately causing reduced overall performance.

[0142] Since Comparative Example 3 does not contain an isolation layer, the outermost layer is only a passivation layer, and the overall color is the color of the passivation layer, which is an uneven micro-color. The passivation layer does not have the function of stabilizing the friction coefficient, resulting in the overall performance failing to meet the requirements.

[0143] In Comparative Example 4, since the isolation layer does not contain polytetrafluoroethylene, the function of the isolation layer to stabilize the friction coefficient is weakened, resulting in the overall friction coefficient exceeding the standard.

[0144] In Comparative Example 5, since the isolation layer does not contain trimethoxymethylsilane, the function of the isolation layer in stabilizing the friction coefficient and the functions of the salt spray test and the sulfur dioxide test are weakened, resulting in the overall performance failing to meet the requirements.

[0145] In Comparative Example 6, since the isolation layer does not contain aluminum powder, the isolation color loses its silvery white color, and the function of balancing the electrode potential when different metals contact is weakened, resulting in the overall color being an uneven micro-color of the passivation layer. The performance of the salt spray test and the sulfur dioxide test is greatly reduced and does not meet the requirements.

[0146] In summary, arranging a galvanized layer, a passivation layer and an isolation layer on the surface of steel fasteners, with the galvanized layer and the passivation layer as the bottom layer, can improve the rust resistance and adhesion of steel fasteners. The isolation layer is coated on the passivation layer. The silver isolation layer contains friction coefficient stabilizing components and has excellent adhesion and friction coefficient stability. When the fasteners are tightened on aluminum alloy or stainless steel parts, the isolation layer isolates the steel fasteners from the aluminum alloy or stainless steel parts, thereby avoiding contact corrosion. At the same time, the stable friction coefficient ensures the fastening force.

[0147] Among them, in the passivation layer, chromium trichloride and oxalic acid will undergo a complex reaction to generate chromium oxalate, which is the main component of the passivation film. Sodium nitrate plays a role in accelerating the passivation reaction and accelerating the film formation, so that the passivation layer can be formed. Cobalt sulfate makes the passivation layer have good corrosion resistance. The complexation rate is increased by complexing chromium trichloride with oxalic acid, thereby increasing the thickness of the passivation film. The passivation reacts quickly by catalysis of sodium nitrate. The acidity of the passivation reaction is reduced by citric acid, so that the passivation film is dissolved while the passivation agent reacts quickly to generate a thick film. Under this dynamic balance, a loose passivation film structure is finally generated.

[0148] In the isolation layer, trimethoxymethylsilane is the main film-forming agent and the main component of the isolation layer formed on the surface of the part. Its main function is to ensure a certain thickness to achieve isolation and rust prevention effects. At the same time, as a component that stabilizes the friction coefficient, it provides a carrier for other friction coefficient stabilizing components. Polytetrafluoroethylene (PTFE) is a friction coefficient regulating component. The friction coefficient of trimethoxymethylsilane is high, and the friction coefficient of polytetrafluoroethylene (PTFE) is low. Through the adjustment of the two components, the friction coefficient of the isolation layer formed on the surface of the part can be kept stable. The function of the silicone leveling agent is to ensure that the thickness of the isolation layer is uniform and the appearance is smooth. The main function of the aluminum paste is to adjust the appearance color of the isolation layer, and at the same time, it plays a role in adjusting the electrode potential of the isolation layer. Further reduce the contact corrosion of steel fasteners.

[0149] The passivating agent forms a passivation film on the galvanized layer. The passivation film can increase the rust resistance of the galvanized layer, that is, improve the corrosion resistance of the steel fasteners. In the present application, due to the presence of citric acid, the dense passivation film is dissolved into a loose non-dense film layer, thereby improving the adhesion of the isolation agent on the passivation film. The formed isolation layer is mutually infiltrated and compounded with the galvanized layer and the passivation layer, rather than a simply superimposed film layer, which further improves the isolation and rust prevention effects.

[0150] In the description of this specification, the description with reference to the terms "one embodiment / method", "some embodiments / methods", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment / method or example are included in at least one embodiment / method or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment / method or example. Moreover, the specific features, structures, materials or characteristics described may be combined in a suitable manner in any one or more embodiments / methods or examples. In addition, those skilled in the art may combine and combine the different embodiments / methods or examples described in this specification and the features of the different embodiments / methods or examples, unless they are contradictory.

[0151] It should be noted that, in the present application, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements not only includes those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements defined by the sentence "including one..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements. In the present application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly specified. The above is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. The various modifications to these embodiments will be obvious to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Thus, the present application will not be limited to the embodiments shown herein but will be accorded the widest scope consistent with the principles and novel features claimed herein.

Claims

1. A steel fastener, characterized in that: It comprises a steel fastener body and a galvanized layer, a passivation layer and an isolation layer arranged on the surface of the steel fastener body from the inside to the outside, wherein: The material of the passivation layer includes chromium trichloride, oxalic acid, sodium nitrate, cobalt sulfate and citric acid; The materials of the isolation layer include trimethoxymethylsilane, polytetrafluoroethylene, organic silicon leveling agent and aluminum powder.

2. The steel fastener according to claim 1, characterized in that: In the material of the passivation layer, the mass ratio of chromium trichloride, oxalic acid, sodium nitrate, cobalt sulfate and citric acid is (25-35): (50-60): (3-5): (8-12): (1-3).

3. The steel fastener according to claim 1, characterized in that: In the material of the isolation layer, the mass ratio of trimethoxymethylsilane, polytetrafluoroethylene, organic silicon leveling agent and aluminum powder is (45-50): (3-8): (15-20): (4-6).

4. The steel fastener according to claim 1, characterized in that: The thickness of the zinc coating is 10 to 12 μm; and / or, The thickness of the passivation layer is 2 to 3 μm; and / or, The thickness of the isolation layer is 4-6 μm.

5. A method for processing a steel fastener according to any one of claims 1 to 4, characterized in that: The following steps are involved: The steel fastener body is subjected to galvanizing treatment to obtain a steel fastener body containing a galvanized layer; preparing the material of the passivation layer into a passivation layer slurry; Dipping the steel fastener body containing the galvanized layer into the passivation layer slurry to form the passivation layer, thereby obtaining the steel fastener body containing the passivation layer; preparing the material of the isolation layer into isolation layer slurry; The steel fastener body containing the passivation layer is immersed in the isolation layer slurry to form the isolation layer, thereby obtaining the steel fastener.

6. The method for processing a steel fastener according to claim 5, characterized in that: The steel fastener body containing the galvanized layer is immersed in the passivation layer slurry to form a passivation layer, thereby obtaining a steel fastener body containing the passivation layer: The immersion time is 1 to 2.5 minutes.

7. The method for processing a steel fastener according to claim 5, characterized in that: The steel fastener body containing the passivation layer is immersed in the isolation layer slurry to form the isolation layer, and the steel fastener comprises: Dipping the steel fastener body containing the passivation layer into the isolation layer slurry to form a first wet isolation layer, thereby obtaining the steel fastener body containing the first wet isolation layer; Centrifuging and drying the steel fastener body containing the first wet isolation layer to form a first dry isolation layer, thereby obtaining a steel fastener body containing the first dry isolation layer; Dipping the steel fastener body containing the first dry isolation layer into the isolation layer slurry to form a second wet isolation layer, thereby obtaining the steel fastener body containing the second wet isolation layer; The steel fastener body containing the second wet isolation layer is centrifuged and dried to form a second dry isolation layer, thereby obtaining the steel fastener body.

8. The method for processing a steel fastener according to claim 7, characterized in that: The immersion time is 0.5 to 2 minutes; and / or, The centrifugal speed is 200-400 r / min; and / or, The centrifugation time is 0.5 to 2 minutes; and / or, The baking temperature is 150-200°C; and / or, The baking time is 15 to 45 minutes.

9. A component, characterized in that: It comprises a steel fastener as described in any one of claims 1 to 4, or a steel fastener made by the processing method of a steel fastener as described in any one of claims 5 to 8.

10. An automobile, characterized in that: Comprising the part as claimed in claim 9.