Assembly and application of iron-based hydrogen production prototype machine for efficiently electrolyzing water

The iron-based electrocatalyst was prepared by electrodeposition method and the high-efficiency electrolytic hydrogen production prototype was assembled, which solved the problem of low oxygen evolution reaction efficiency, achieved high hydrogen yield and simple preparation, and demonstrated excellent engineering application prospects.

CN118957630APending Publication Date: 2024-11-15UNIV OF ELECTRONICS SCI & TECH OF CHINA
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411027504.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the existing electrolytic hydrogen production technology, the slow kinetics of the oxygen evolution reaction lead to insufficient gas precipitation, slow precipitation rate, making it difficult to improve the efficiency of electrocatalytic decomposition of water.

Method used

The iron-based electrocatalyst is prepared by electrodeposition method, and the stainless steel mesh is used as the anode and nickel mesh is used as the cathode. The proton exchange and electrolyte barrier are achieved through the proton exchange membrane, and the iron-based oxygen evolution reaction electrocatalyst and the Rainey nickel cathode electrocatalyst are fixed. High-efficiency iron-based electrolytic hydrogen production prototype.

Benefits of technology

High gas output is achieved at low electrode area, simplifying the preparation process, and efficient hydrogen production at room temperature, showing excellent engineering application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957630A_ABST
    Figure CN118957630A_ABST
Patent Text Reader

Abstract

The invention discloses an assembly method and application of a simple and efficient iron-based electrocatalyst oxygen production and Raney nickel hydrogen production efficient prototype machine. The assembly method comprises the following steps: (1) dissolving ferric chloride hexahydrate and sodium thiosulfate pentahydrate in deionized water, and uniformly stirring to obtain an electrodeposition electrolyte; (2) preparing an anode of the prototype machine for producing hydrogen by electrolyzing water by adopting an electro-deposition method; and (3) assembling the prototype machine for producing hydrogen by electrolyzing water by using the nickel net sprayed with Raney nickel as a cathode and the iron-based stainless steel net as an anode. The prepared iron-based water electrolysis hydrogen production prototype machine adopts a simple assembly method, can continuously operate at normal temperature, can generate high hydrogen evolution amount of 100 milliliters per minute by adopting a small-size conductive net, and shows excellent engineering application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of hydrogen production by electrolysis of water, and specifically relates to an assembly method and application of an efficient prototype machine for producing oxygen by using an iron-based electrocatalyst and producing hydrogen by using Raney nickel. Background Art

[0002] With the rapid development of social economy, the huge energy demand has led to large-scale exploitation of fossil fuels. In order to solve the problems of environmental pollution and depletion of non-renewable resources, the development of renewable, green, clean, low-cost, stable and efficient energy substitutes has become an inevitable choice. Hydrogen energy, as a secondary energy with abundant sources, low carbon emissions, high energy density, high calorific value and wide application, can break through the external environmental constraints of clean energy such as solar energy and wind energy, and greatly improve the stability of energy utilization. As the most promising hydrogen production method at present, hydrogen is mainly produced by storing, transporting and converting the generated electrical energy. Hydrogen production by water electrolysis is divided into two main half-reactions, namely the hydrogen evolution reaction occurring at the cathode end and the oxygen evolution reaction occurring at the anode. However, due to the slow kinetics of the oxygen evolution reaction, the amount of gas evolution from water electrolysis is insufficient and the evolution rate is slow, which poses a major challenge to improving the efficiency of electrocatalytic water decomposition. Therefore, it is crucial to prepare a simple and efficient water electrolysis prototype.

[0003] In recent years, metal chalcogenides (sulfides, selenides and tellurides, etc.) have been widely studied due to their rich pores, stronger conductivity and catalytic activity. Electrodeposition is a method that uses anode dissolution to obtain metal ions, which then react with an electrolyte medium. It can operate continuously and is suitable for directly loading catalysts on a conductive substrate, and can be widely used in industrial production. Nickel mesh and stainless steel mesh are used as conductive substrates for the cathode and anode, respectively. Both are resistant to corrosion in strong alkaline environments, which provides a guarantee for conductivity. Nowadays, in order to achieve high hydrogen evolution, a large conductive substrate area is generally required. Therefore, how to achieve high gas production at a low electrode area requires further exploration of electrocatalysts. Summary of the invention

[0004] In order to overcome the above-mentioned deficiencies of the prior art, the present invention provides a simple and efficient assembly method of an iron-based water electrolysis hydrogen production prototype.

[0005] To achieve the above object, the technical solution of the present invention is as follows:

[0006] A method for assembling a high-efficiency iron-based water electrolysis hydrogen production prototype comprises the following steps:

[0007] Step 1: Preparation of electrolyte for electrodeposition method: Dissolve ferric chloride hexahydrate and sodium thiosulfate pentahydrate in deionized water and stir well;

[0008] Step 2: Preparation of the anode of the prototype machine for hydrogen production by electrolysis of water: Use the cleaned stainless steel mesh as the anode, the carbon rod as the cathode, and the above mixed solution as the electrolyte, and use a DC power supply to perform electrodeposition for a period of time at a preset voltage. Then wash the stainless steel mesh with deionized water and finally put it in an oven to dry.

[0009] Step 3: Assembly of the prototype machine for hydrogen production by electrolysis of water: electrolyzed water and alkaline electrolyte of a certain concentration are respectively placed in the glass containers at the positive and negative electrodes in the sealed H-type electrolytic cell or electrolytic tank; proton exchange and electrolyte barrier are achieved by using a proton exchange membrane; the iron-based oxygen evolution reaction electrocatalyst prepared in step 2 is fixed on the anode electrode clamp, and the nickel mesh sprayed with Raney nickel is fixed on the cathode electrode clamp; the cathode and anode are respectively connected to the positive and negative electrodes of an external DC power supply; and gas ducts for oxygen and hydrogen are connected from the cathode and anode top covers.

[0010] Step 4: Place a graduated measuring cylinder filled with water upside down in a large beaker of water, and place the outlet end of the hydrogen tube into the bottom of the measuring cylinder to collect, test and record the hydrogen production rate.

[0011] As a preferred embodiment, the preset voltage in step 2 is 3 to 6V.

[0012] As a preferred embodiment, the electrodeposition time in step 2 is 10 to 60 seconds.

[0013] As a preferred embodiment, in step 3, the sizes of the stainless steel mesh and the nickel mesh are consistent.

[0014] As a preferred embodiment, the alkaline electrolyte in step 3 is potassium hydroxide, sodium hydroxide, etc.

[0015] As a preferred embodiment, the concentration of potassium hydroxide and sodium hydroxide in the neutral alkaline electrolyte in step 3 is 10-50%.

[0016] Compared with the prior art, the advantages of the present invention are:

[0017] 1. The present invention adopts a simpler, time-saving and room-temperature electrodeposition method to prepare the anode of the hydrogen production prototype.

[0018] 2. The present invention can achieve a high hydrogen production of 100 ml / min by using a small-sized conductive mesh.

[0019] 3. The iron-based water electrolysis hydrogen production prototype of the present invention is simple to assemble and operates at room temperature.

[0020] 4. The present invention shows excellent engineering application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 A schematic diagram of the connection method of a high-efficiency iron-based water electrolysis hydrogen production prototype machine prepared in accordance with an embodiment of the present invention; DETAILED DESCRIPTION

[0022] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0023] Example

[0024] A simple and efficient assembly method of an iron-based water electrolysis hydrogen production prototype comprises the following steps:

[0025] Step 1: Preparation of electrolyte for electrodeposition method: Dissolve ferric chloride hexahydrate and sodium thiosulfate pentahydrate in deionized water and stir well;

[0026] Step 2: Preparation of the anode of the prototype machine for hydrogen production by electrolysis of water: Use the cleaned stainless steel mesh as the anode, the carbon rod as the cathode, and the above mixed solution as the electrolyte, and use a DC power supply to perform electrodeposition for 40 seconds at a preset voltage of 5V. Then wash the stainless steel mesh with deionized water and finally put it in an oven to dry.

[0027] Step 3: Assembly of the prototype machine for hydrogen production by electrolysis of water: electrolyzed water and a certain concentration of alkaline 30% potassium hydroxide electrolyte are respectively placed in the glass containers at the positive and negative electrodes in the sealed H-type electrolytic cell or electrolytic tank; a proton exchange membrane is used to achieve proton exchange and electrolyte barrier; the iron-based oxygen evolution reaction electrocatalyst prepared in step 2 is fixed on the anode electrode clamp, and a nickel mesh sprayed with Raney nickel of the same size as the stainless steel is fixed on the cathode electrode clamp; the cathode and anode are respectively connected to the positive and negative electrodes of an external DC power supply; and the gas ducts for oxygen and hydrogen are connected from the cathode and anode top covers.

[0028] Step 4: Place a graduated measuring cylinder filled with water upside down in a large beaker of water, and place the outlet end of the hydrogen tube into the bottom of the measuring cylinder to collect, test and record the hydrogen production rate.

[0029] The iron-based prototype obtained can be directly used in hydrogen production by electrolysis of water. By using iron-based sulfide deposited on stainless steel as an anode electrocatalyst and a nickel mesh loaded with Raney nickel as a cathode electrocatalyst, a higher hydrogen production can be achieved, showing its excellent engineering application prospects.

[0030] Example 1

[0031] A simple and efficient assembly method of an iron-based water electrolysis hydrogen production prototype comprises the following steps:

[0032] Step 1: Preparation of electrolyte for electrodeposition method: Dissolve ferric chloride hexahydrate and sodium thiosulfate pentahydrate in deionized water and stir well;

[0033] Step 2: Preparation of the anode of the prototype machine for hydrogen production by electrolysis of water: Use the cleaned stainless steel mesh as the anode, the carbon rod as the cathode, and the above mixed solution as the electrolyte, and use a DC power supply to perform electrodeposition for 40 seconds at a preset voltage of 5V. Then wash the stainless steel mesh with deionized water and finally put it in an oven to dry.

[0034] Step 3: Assembly of the prototype machine for hydrogen production by electrolysis of water: electrolyzed water and 30% alkaline potassium hydroxide electrolyte are respectively placed in the glass containers at the positive and negative electrodes in a sealed H-type electrolytic cell or electrolytic tank, and proton exchange and electrolyte barrier are achieved by using a proton exchange membrane; the iron-based oxygen evolution reaction electrocatalyst prepared in step 2 is fixed on the anode electrode clamp, and a nickel mesh sprayed with Raney nickel of the same size as the stainless steel is fixed on the cathode electrode clamp; the cathode and anode are respectively connected to the positive and negative electrodes of an external DC power supply; and gas ducts for oxygen and hydrogen are connected from the cathode and anode top covers.

[0035] Step 4: Place a graduated measuring cylinder filled with water upside down in a large beaker of water, and place the outlet end of the hydrogen tube into the bottom of the measuring cylinder to collect, test and record the hydrogen production rate.

[0036] The iron-based prototype obtained can be directly used in hydrogen production by electrolysis of water. By using iron-based sulfide deposited on stainless steel as an anode electrocatalyst and a nickel mesh loaded with Raney nickel as a cathode electrocatalyst, a higher hydrogen production can be achieved, showing its excellent engineering application prospects.

[0037] Example 2

[0038] A simple and efficient assembly method of an iron-based water electrolysis hydrogen production prototype comprises the following steps:

[0039] Step 1: Preparation of electrolyte for electrodeposition method: Dissolve ferric chloride hexahydrate and sodium thiosulfate pentahydrate in deionized water and stir well;

[0040] Step 2: Preparation of the anode of the prototype machine for hydrogen production by electrolysis of water: Use the cleaned stainless steel mesh as the anode, the carbon rod as the cathode, and the above mixed solution as the electrolyte, and use a DC power supply to perform electrodeposition for 10 seconds at a preset voltage of 6V. Then wash the stainless steel mesh with deionized water and finally put it in an oven to dry.

[0041] Step 3: Assembly of the prototype machine for hydrogen production by electrolysis of water: electrolyzed water and 10% alkaline potassium hydroxide electrolyte are respectively placed in the glass containers at the positive and negative electrodes in a sealed H-type electrolytic cell or electrolytic tank, and proton exchange and electrolyte barrier are achieved by using a proton exchange membrane; the iron-based oxygen evolution reaction electrocatalyst prepared in step 2 is fixed on the anode electrode clamp, and a nickel mesh sprayed with Raney nickel of the same size as the stainless steel is fixed on the cathode electrode clamp; the cathode and anode are respectively connected to the positive and negative electrodes of an external DC power supply; and gas ducts for oxygen and hydrogen are connected from the cathode and anode top covers.

[0042] Step 4: Place a graduated measuring cylinder filled with water upside down in a large beaker of water, and place the outlet end of the hydrogen tube into the bottom of the measuring cylinder to collect, test and record the hydrogen production rate.

[0043] The iron-based prototype obtained can be directly used in hydrogen production by electrolysis of water. By using iron-based sulfide deposited on stainless steel as an anode electrocatalyst and a nickel mesh loaded with Raney nickel as a cathode electrocatalyst, a higher hydrogen production can be achieved, showing its excellent engineering application prospects.

[0044] Example 3

[0045] A simple and efficient assembly method of an iron-based water electrolysis hydrogen production prototype comprises the following steps:

[0046] Step 1: Preparation of electrolyte for electrodeposition method: Dissolve ferric chloride hexahydrate and sodium thiosulfate pentahydrate in deionized water and stir well;

[0047] Step 2: Preparation of the anode of the prototype machine for hydrogen production by electrolysis of water: Use the cleaned stainless steel mesh as the anode, the carbon rod as the cathode, and the above mixed solution as the electrolyte, and use a DC power supply to perform electrodeposition for 60 seconds at a preset voltage of 3V. Then wash the stainless steel mesh with deionized water and finally put it in an oven to dry.

[0048] Step 3: Assembly of the prototype machine for hydrogen production by electrolysis of water: electrolyzed water and 50% alkaline potassium hydroxide electrolyte are respectively placed in the glass containers at the positive and negative electrodes in a sealed H-type electrolytic cell or electrolytic tank, and proton exchange and electrolyte barrier are achieved by using a proton exchange membrane; the iron-based oxygen evolution reaction electrocatalyst prepared in step 2 is fixed on the anode electrode clamp, and a nickel mesh sprayed with Raney nickel of the same size as the stainless steel is fixed on the cathode electrode clamp; the cathode and anode are respectively connected to the positive and negative electrodes of an external DC power supply; and gas ducts for oxygen and hydrogen are connected from the cathode and anode top covers.

[0049] Step 4: Place a graduated measuring cylinder filled with water upside down in a large beaker of water, and place the outlet end of the hydrogen tube into the bottom of the measuring cylinder to collect, test and record the hydrogen production rate.

[0050] The iron-based prototype obtained can be directly used in hydrogen production by electrolysis of water. By using iron-based sulfide deposited on stainless steel as an anode electrocatalyst and a nickel mesh loaded with Raney nickel as a cathode electrocatalyst, a higher hydrogen production can be achieved, showing its excellent engineering application prospects.

[0051] Example 4

[0052] A simple and efficient assembly method of an iron-based water electrolysis hydrogen production prototype comprises the following steps:

[0053] Step 1: Preparation of electrolyte for electrodeposition method: Dissolve ferric chloride hexahydrate and sodium thiosulfate pentahydrate in deionized water and stir well;

[0054] Step 2: Preparation of the anode of the prototype machine for hydrogen production by electrolysis of water: Use the cleaned stainless steel mesh as the anode, the carbon rod as the cathode, and the above mixed solution as the electrolyte, and use a DC power supply to perform electrodeposition for 40 seconds at a preset voltage of 5V. Then wash the stainless steel mesh with deionized water and finally put it in an oven to dry.

[0055] Step 3: Assembly of the prototype machine for hydrogen production by electrolysis of water: electrolyzed water and 30% alkaline sodium hydroxide electrolyte are respectively placed in the glass containers at the positive and negative electrodes in a sealed H-type electrolytic cell or electrolytic tank, and proton exchange and electrolyte barrier are achieved by using a proton exchange membrane; the iron-based oxygen evolution reaction electrocatalyst prepared in step 2 is fixed on the anode electrode clamp, and a nickel mesh sprayed with Raney nickel of the same size as the stainless steel is fixed on the cathode electrode clamp; the cathode and anode are respectively connected to the positive and negative electrodes of an external DC power supply; and gas ducts for oxygen and hydrogen are connected from the cathode and anode top covers.

[0056] Step 4: Place a graduated measuring cylinder filled with water upside down in a large beaker of water, and place the outlet end of the hydrogen tube into the bottom of the measuring cylinder to collect, test and record the hydrogen production rate.

[0057] The iron-based prototype obtained can be directly used in hydrogen production by electrolysis of water. By using iron-based sulfide deposited on stainless steel as an anode electrocatalyst and a nickel mesh loaded with Raney nickel as a cathode electrocatalyst, a higher hydrogen production can be achieved, showing its excellent engineering application prospects.

[0058] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for preparing a high-efficiency iron-based water electrolysis hydrogen production prototype, characterized in that The steps include: Step 1: Preparation of electrolyte for electrodeposition method: Dissolve ferric chloride hexahydrate and sodium thiosulfate pentahydrate in deionized water and stir well; Step 2: Preparation of the anode of the prototype machine for hydrogen production by electrolysis of water: Use the cleaned stainless steel mesh as the anode, the carbon rod as the cathode, and the above mixed solution as the electrolyte, and use a DC power supply to perform electrodeposition for a period of time at a preset voltage. Then wash the stainless steel mesh with deionized water and finally put it in an oven to dry. Step 3: Assembly of the prototype machine for hydrogen production by electrolysis of water: Place an alkaline electrolyte of a certain concentration for water electrolysis in the glass containers at the anode and cathode in a sealed H-type electrolytic cell or electrolyzer, and use a proton exchange membrane to achieve proton exchange and block the electrolyte; fix the iron-based oxygen evolution reaction electrocatalyst prepared in step 2 on the anode electrode clamp, and fix the nickel mesh sprayed with Raney nickel on the cathode electrode clamp; connect the cathode and anode to the positive and negative electrodes of an external DC power supply respectively; connect the gas ducts for oxygen and hydrogen from the cathode and anode top covers. Step 4: Place a graduated measuring cylinder filled with water upside down in a large beaker of water, and place the outlet end of the hydrogen tube into the bottom of the measuring cylinder to collect, test and record the hydrogen production rate.

2. The method for preparing a high-efficiency iron-based water electrolysis hydrogen production prototype according to claim 1, characterized in that: The preset voltage in step 2 is 3 to 6V.

3. The method for preparing a high-efficiency iron-based water electrolysis hydrogen production prototype according to claim 1, characterized in that: The electrodeposition time in step 2 is 10 to 60 seconds.

4. The method for preparing a high-efficiency iron-based water electrolysis hydrogen production prototype according to claim 1, characterized in that: In step 3, the sizes of the stainless steel mesh and the nickel mesh are the same.

5. The method for preparing a high-efficiency iron-based water electrolysis hydrogen production prototype according to claim 1, characterized in that: In step 3, the alkaline electrolyte is potassium hydroxide, sodium hydroxide, etc.

6. The method for preparing a high-efficiency iron-based water electrolysis hydrogen production prototype according to claim 1, characterized in that: In step 3, the concentration of potassium hydroxide and sodium hydroxide in the alkaline electrolyte is 10-50%.

7. The high-efficiency iron-based water electrolysis hydrogen production prototype obtained by the method described in any one of claims 1 to 6 can be used as a unit, and N units can be connected in parallel to obtain N times the hydrogen production.

8. The high-efficiency iron-based water electrolysis hydrogen production prototype according to claim 7 is characterized by: Each unit can achieve a hydrogen production rate greater than 100 ml per minute, demonstrating broad prospects for industrial applications.

Citation Information

Cited By

  • A post-treatment method for preventing coating from falling off of a raney nickel electrode under reverse current

    CN122751293A

  • A post-treatment method for preventing coating from falling off of a raney nickel electrode under reverse current

    CN122751293B