Self-supporting electrode and preparation method and application thereof

Through the preparation method of self-support electrodes, metal oxide coatings are formed using pretreatment of metal substrates and physical and chemical means, which solves the problems of complex traditional electrode preparation processes and low catalyst utilization, and achieves efficient CO2 reduction catalysis and simplified process , suitable for a variety of electrochemical applications.

CN118957631APending Publication Date: 2024-11-15DALIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411050226.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the existing CO2 reduction electrocatalytic reaction, the preparation process of traditional gas diffusion electrodes is complex and requires strict slurry uniformity, resulting in a long process route and is not suitable for efficient catalyst utilization, and the Faraday efficiency of C2 products is low.

Method used

The preparation method of self-supporting electrodes is adopted to induce nucleation through pretreatment of metal substrates and physical and chemical means to form metal oxide coatings, simplify the process route, improve the catalyst utilization and hydrophobicity, avoid spraying steps, and enhance catalytic performance.

Benefits of technology

The high specific surface area and high hydrophobicity of the self-supported electrode are achieved, the utilization rate of the catalyst and the Faraday efficiency of C2H4 are improved, the preparation process is simplified, and the preparation process is suitable for water electrolysis, fuel cells, sensors and carbon dioxide electrochemical reduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957631A_ABST
    Figure CN118957631A_ABST
Patent Text Reader

Abstract

The invention relates to a self-supporting electrode, a preparation method and application thereof. The self-supporting electrode comprises a metal substrate and a metal oxide coating on the surface of the metal substrate. After the surface of the substrate is etched under the ultrasonic condition, a metal oxide coating electrocatalyst is prepared through low-temperature pyrolysis dehydration, and the self-supporting electrode is obtained. The prepared self-supporting electrode has the advantages of high catalyst utilization rate, high hydrophobicity and the like. The prepared self-supporting electrode can be used for reaction devices in water electrolysis, fuel cells, sensors and carbon dioxide electrochemical reduction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of electrochemical catalysis, and specifically relates to a self-supporting electrode and a preparation method and application thereof. The prepared self-supporting electrode can be used in water electrolysis, fuel cells, sensors, and reaction devices for electrochemical reduction of carbon dioxide. Background Art

[0002] The massive emission of CO2 has led to severe climate and environmental problems such as global temperature rise, sea level rise, and ocean acidification. The country has introduced a number of policies to encourage and support measures such as CO2 recovery, utilization and conversion in order to achieve the dual carbon goal. Among them, due to the advantages of mild operating conditions and easy control of the reaction process by changing the applied potential, the electrocatalytic CO2 reduction (CO2RR) is an important solution strategy for converting CO2 into fuel chemicals. The electrocatalytic CO2 reaction is relatively complex and competes fiercely with the side reaction hydrogen evolution (HER). The main products of the reaction are CO, CH4, C2H4, C2H6 and C3H8. Compared with C1 products, C2 products have greater economic benefits, among which C2H4 is an important basic raw material for petrochemicals. The industry regards C2H4 production capacity as an important indicator of the development level of a country's petrochemical industry. There are many types of C2H4 derivative products, accounting for more than 75% of the total global petrochemical products. At present, the research on CO2RR mainly focuses on the traditional gas diffusion electrode, which is usually prepared by mixing the catalyst with the dispersant to form a uniform slurry, and spraying or dripping the slurry on the surface of the gas diffusion layer to obtain the gas diffusion electrode. Its preparation process is long and has strict requirements on the uniformity of the slurry. The self-supporting electrode can be used as a working electrode for testing by surface modification of its own material, which greatly shortens the process route. Therefore, the self-supporting electrode has become a new research hotspot in the field of electrocatalytic CO2 reduction.

[0003] There are many studies on the surface modification of self-supporting electrodes. The commonly used preparation process is through electrochemical methods. Philipp Grosse et al. (Philipp Grosse, et al. Angewandte Chemie International Edition, 2018, 57 (21): 6192-6197) electropolished the surface-cleaned Cu foil in H3PO4 solution, and further electrochemically anodized Cu nanocubes in KCl electrolyte to obtain Cu-based self-supporting electrodes, which advantageously exposed specific crystal faces and improved the Faraday efficiency of C2H4. Chang Liu et al. (Chang Liu, et al. ACS Applied Materials & Interfaces, 2022, 14 (18): 20953-20961) mechanically polished the Cu foil, and then ultrasonically washed it with hydrochloric acid, deionized water, acetone and ethanol in turn. The cleaned Cu foil was used as the working electrode for electrochemical anodization in Na2HPO4 electrolyte, and nano-dendritic Cu was prepared on the surface of the Cu foil, which enhanced the adsorption of key intermediates and promoted CC coupling. Summary of the invention

[0004] The purpose of the present invention is to provide a self-supporting electrode and its preparation method and application in view of the deficiencies of the prior art. The prepared self-supporting electrode can be used in water electrolysis, fuel cells, sensors, and reaction devices for electrochemical reduction of carbon dioxide.

[0005] The technical solution of the present invention is:

[0006] A self-supporting electrode comprises a metal substrate and a metal oxide coating (electrocatalyst) on the surface of the metal substrate.

[0007] The metal substrate described in the present invention is metal foil or foam metal, and the metal is at least one of Pt, Ir, Pd, Au, Ru, Rh, Ag, Cu, Fe, Co, Ni, and Mn.

[0008] The metal of the metal oxide coating in the present invention is at least one of Pt, Ir, Pd, Au, Ru, Rh, Ag, Cu, Fe, Co, Ni, and Mn.

[0009] The thickness of the metal substrate in the present invention is 0.02-10 mm, preferably 0.02-2 mm, more preferably 0.02-1 mm, and further preferably 0.02-0.5 mm.

[0010] The thickness of the metal oxide coating in the present invention is 1-10 μm, preferably 1-8 μm, and more preferably 2-5 μm.

[0011] Another object of the present invention is to provide a method for preparing the above-mentioned self-supporting electrode, the preparation method comprising the following steps:

[0012] (1) Pretreatment of metal substrate

[0013] The metal substrate is placed in a mixed solvent of an organic solvent and water for ultrasonic treatment for 10-60 minutes, then rinsed with water and ethanol in sequence, dried and placed in an acid solution for 15-60 minutes to remove the oxide layer on the surface, thereby obtaining a pretreated substrate.

[0014] (2) Preparation of self-supporting electrodes

[0015] The pretreated substrate is placed in an alkaline solution and treated by physical means at the same time, nucleation is induced on the surface of the substrate by physical and chemical means, and then allowed to stand for 0-240 minutes (preferably 30-90 minutes) to etch the surface. After being taken out, it is rinsed with deionized water, dried, and heat treated at 150-750°C (preferably 200-300°C) for 30-120 minutes in a certain atmosphere to obtain a self-supporting electrode covered with a metal oxide coating.

[0016] In step (1) of the present invention, the organic solvent is at least one of methanol, ethanol, propanol, isopropanol, butanol, ethylene glycol, propylene glycol, ether, chloroform, cyclohexane, toluene and acetone. The volume ratio of the organic solvent to water in the mixed solvent of the organic solvent and water is 2:1-4:1. When the organic solvent is a mixture of acetone and ethanol, the volume ratio of acetone to ethanol is 1:1-3:1.

[0017] In step (1) of the present invention, the ultrasonic power is 400-600W.

[0018] In step (1) of the present invention, the acid is at least one of formic acid, acetic acid, phosphoric acid, hydrochloric acid and sulfuric acid. The concentration of the acid solution is 0.01-10 mol / L, preferably 0.05-0.20 mol / L.

[0019] In step (2) of the present invention, the alkali is at least one of sodium hydroxide, potassium hydroxide, calcium hydroxide, lithium hydroxide, ammonia water, potassium carbonate, potassium bicarbonate, sodium carbonate, and sodium bicarbonate. The concentration of the alkali solution is 0.01-10 mol / L, preferably 0.01-0.10 mol / L.

[0020] In step (2) of the present invention, the physical means is at least one of laser, ultrasound and microwave. When the physical means is ultrasound, the ultrasound time is 15-60 minutes and the ultrasound power is 60-90 W. That is, after etching the substrate surface under ultrasound conditions, the metal oxide coating is prepared by low-temperature thermal dehydration.

[0021] In step (2) of the present invention, the atmosphere is at least one of helium, argon, nitrogen, hydrogen, air, and carbon monoxide.

[0022] Another object of the present invention is to provide the application of the above self-supporting electrode in water electrolysis, fuel cells, sensors, and electrochemical reduction of carbon dioxide.

[0023] The present invention first etches the substrate in situ in an etching solution without a surfactant to obtain a nucleation site, further epitaxially grows / deposit to obtain a self-supporting working electrode with a metal hydroxide covering the substrate, and then obtains a metal oxide coating by heat treatment, avoiding the spraying step, and developing a new self-supporting electrode structure and electrode preparation process. By etching the surface of the substrate, the roughness of the substrate surface is increased, and the utilization rate of the catalyst is improved; the metal hydroxide is dehydrated by low-temperature pyrolysis of the substrate to improve the hydrophilicity and hydrophobicity of the electrode surface. The self-supporting electrode prepared by the present invention has the advantages of high catalyst utilization and high hydrophobicity. The prepared self-supporting electrode can be used in water electrolysis, fuel cells, sensors, and reaction devices for electrochemical reduction of carbon dioxide.

[0024] Compared with the prior art, the present invention has the following advantages:

[0025] 1) The self-supporting electrode prepared by the present invention has a large specific surface area and a high catalyst utilization rate;

[0026] 2) The self-supporting electrode prepared by the present invention has a high degree of hydrophobicity on the surface;

[0027] 3) The preparation method of the self-supporting electrode described in the present invention is simple, feasible, and easy to process and scale up, providing a new technical route for the preparation of the self-supporting electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The present invention is attached Figure 7 width,

[0029] Figure 1 The scanning electron microscope (SEM) images of the self-supporting electrode before and after pretreatment in Example 1;

[0030] Figure 2 The SEM images of the self-supporting electrode before and after the metal oxide coating is prepared in Example 1;

[0031] Figure 3 The SEM images of the self-supporting electrodes after the metal oxide coating was prepared under static / ultrasonic induction conditions in Comparative Example 1 and Example 1;

[0032] Figure 4 is the X-ray diffraction (XRD) spectrum of the self-supporting electrode prepared by ultrasonic induction in Example 1;

[0033] Figure 5is the Faraday efficiency of CO2RR gas phase products of the self-supporting electrode prepared by ultrasonic induction in Example 1 in an H-type electrolytic cell;

[0034] Figure 6 The SEM images of the self-supporting electrodes prepared at different standing times after ultrasonic induction in Example 2, Example 3, Example 1 and Example 4;

[0035] Figure 7 These are contact angle photographs of the self-supporting electrodes prepared at different standing times after ultrasonic induction in Examples 2, 3, 1 and 4. DETAILED DESCRIPTION

[0036] The present invention is further described below in conjunction with embodiments, but the present invention is not limited thereto.

[0037] Example 1

[0038] (1) Substrate pretreatment

[0039] A copper foil (1 cm long, 1 cm wide, and 0.04 mm thick) was placed in a mixed solvent of acetone, ethanol, and water (the volume ratio of acetone, ethanol, and water was 1:1:1) and ultrasonicated (ultrasonic power 500 W) for 30 min. The foil was rinsed with water and ethanol in turn. After drying, the foil was placed in 0.1 M hydrochloric acid for 30 min to remove the oxide layer on the surface. After treatment, the foil was rinsed with deionized water and dried to obtain the pretreated copper foil.

[0040] (2) Preparation of self-supporting electrodes

[0041] The pretreated copper foil was placed in 0.05M NH3·H2O and ultrasonicated (ultrasonic power 80W) for 30 minutes and then allowed to stand for 120 minutes to etch its surface. After being taken out, it was rinsed with deionized water, dried, and heat treated at 250°C for 30 minutes in an Ar atmosphere to obtain a self-supporting electrode with a metal oxide coating.

[0042] The prepared self-supporting electrode is used in a reaction device for electrochemical reduction of carbon dioxide.

[0043] Comparative Example 1

[0044] (1) Substrate pretreatment

[0045] A copper foil (1 cm long, 1 cm wide, and 0.04 mm thick) was placed in a mixed solvent of acetone, ethanol, and water (the volume ratio of acetone, ethanol, and water was 1:1:1) and ultrasonicated (ultrasonic power 500 W) for 30 min. The foil was rinsed with water and ethanol in turn. After drying, the foil was placed in 0.1 M hydrochloric acid for 30 min to remove the oxide layer on the surface. After treatment, the foil was rinsed with deionized water and dried to obtain the pretreated copper foil.

[0046] (2) Preparation of self-supporting electrodes

[0047] The pretreated copper foil was placed in 0.05M NH3·H2O and allowed to stand for 150 minutes to etch its surface. After being taken out, it was rinsed with deionized water, dried, and heat treated at 250°C for 30 minutes in an Ar atmosphere to obtain a self-supporting electrode with a metal oxide coating.

[0048] The prepared self-supporting electrode is used in a reaction device for electrochemical reduction of carbon dioxide.

[0049] Figure 1 The SEM photos of the self-supporting electrode before and after pretreatment in Example 1 show that before pretreatment, there is a natural oxide layer on the surface of the copper foil, and after pretreatment, the surface of the copper foil becomes rough.

[0050] Figure 2 These are SEM photos of the self-supporting electrode before and after the metal oxide coating is prepared in Example 1 (before and after heat treatment), indicating that compared with before heat treatment, after the metal oxide coating is prepared on its surface, the micron-scale texture structure is maintained, and the surface evolves from a nanorod shape to a nanowire structure.

[0051] Figure 3 This is an SEM photograph of the self-supporting electrode after the metal oxide coating is prepared under static conditions in Comparative Example 1 / ultrasonic conditions in Example 1, indicating that compared with the static conditions, after the metal oxide coating is prepared under the physical induction of ultrasound, the surface of the copper foil becomes rough and a micron-scale nanowire network texture structure is formed.

[0052] Figure 4 This is the XRD spectrum of the self-supporting electrode prepared by ultrasonic induction in Example 1, indicating that a metal oxide coating of CuO is formed on the surface of the copper foil.

[0053] Figure 5 The Faraday efficiency of CO2RR gas phase products in the H-type electrolytic cell of the self-supporting electrode prepared by ultrasonic induction in Example 1 is shown in Figure 1. The test conditions are: CO2 flow rate of 20 mL / min, electrolytic cell reaction temperature of 25 ° C, atmospheric pressure, electrolyte: 0.5M KCl aqueous solution. As the electrolysis voltage increases, the Faraday efficiency of ethylene increases first and then decreases. At -1.2 V vs. RHE, the maximum Faraday efficiency of ethylene is 50.2%.

[0054] Example 2

[0055] (1) Pretreatment of substrate

[0056] A copper foil (1 cm long, 1 cm wide, and 0.04 mm thick) was placed in a mixed solvent of acetone, ethanol, and water (the volume ratio of acetone, ethanol, and water was 1:1:1) and ultrasonicated (ultrasonic power 500 W) for 30 min. The foil was rinsed with water and ethanol in turn. After drying, the foil was placed in 0.1 M hydrochloric acid for 30 min to remove the oxide layer on the surface. After treatment, the foil was rinsed with deionized water and dried to obtain the pretreated copper foil.

[0057] (2) Preparation of self-supporting electrodes

[0058] The pretreated copper foil was placed in 0.05M NH3·H2O and ultrasonicated (ultrasonic power 80W) for 30 minutes, then allowed to stand for 0 minutes to etch its surface. After being taken out, it was rinsed with deionized water, dried, and heat treated at 250°C for 30 minutes in an Ar atmosphere to obtain a self-supporting electrode with a metal oxide coating.

[0059] The prepared self-supporting electrode is used in a reaction device for electrochemical reduction of carbon dioxide.

[0060] Example 3

[0061] (1) Substrate pretreatment

[0062] A copper foil (1 cm long, 1 cm wide, and 0.04 mm thick) was placed in a mixed solvent of acetone, ethanol, and water (the volume ratio of acetone, ethanol, and water was 1:1:1) and ultrasonicated (ultrasonic power 500 W) for 30 min. The foil was rinsed with water and ethanol in turn. After drying, the foil was placed in 0.1 M hydrochloric acid for 30 min to remove the oxide layer on the surface. After treatment, the foil was rinsed with deionized water and dried to obtain the pretreated copper foil.

[0063] (2) Preparation of self-supporting electrodes

[0064] The pretreated copper foil was placed in 0.05M NH3·H2O and ultrasonicated (ultrasonic power 80W) for 30 minutes and then allowed to stand for 60 minutes to etch its surface. After being taken out, it was rinsed with deionized water, dried, and heat treated at 250°C for 30 minutes in an Ar atmosphere to obtain a self-supporting electrode with a metal oxide coating.

[0065] The prepared self-supporting electrode is used in a reaction device for electrochemical reduction of carbon dioxide.

[0066] Example 4

[0067] (1) Substrate pretreatment

[0068] A copper foil (1 cm long, 1 cm wide, and 0.04 mm thick) was placed in a mixed solvent of acetone, ethanol, and water (the volume ratio of acetone, ethanol, and water was 1:1:1) and ultrasonicated (ultrasonic power 500 W) for 30 min. The foil was rinsed with water and ethanol in turn. After drying, the foil was placed in 0.1 M hydrochloric acid for 30 min to remove the oxide layer on the surface. After treatment, the foil was rinsed with deionized water and dried to obtain the pretreated copper foil.

[0069] (2) Preparation of self-supporting electrodes

[0070] The pretreated copper foil was placed in 0.05M NH3·H2O and ultrasonicated (ultrasonic power 80W) for 30 minutes and then allowed to stand for 180 minutes to etch its surface. After being taken out, it was rinsed with deionized water, dried, and heat treated at 250°C in an Ar atmosphere for 30 minutes to obtain a self-supporting electrode with a metal oxide coating.

[0071] The prepared self-supporting electrode is used in a reaction device for electrochemical reduction of carbon dioxide.

[0072] Figure 6 The SEM images of the self-supporting electrodes prepared at different standing times after ultrasonic induction in Examples 2, 3, 1 and 4 show that the CuO nanowires on the surface of the copper foil gradually grow to be dense with increasing standing time.

[0073] Figure 7 These are photos of the contact angles of the self-supporting electrodes prepared at different standing times after ultrasonic induction in Examples 2, 3, 1, and 4. It is apparent that as the standing time increases, the contact angle of the self-supporting electrode first increases and then decreases. When the standing time is 2 hours, the maximum contact angle is 149.2°.

[0074] Example 5

[0075] (1) Substrate pretreatment

[0076] An iron foil (1 cm long, 1 cm wide, and 0.03 mm thick) was placed in a mixed solvent of acetone, ethanol, and water (the volume ratio of acetone, ethanol, and water was 1:1:1) and ultrasonicated (ultrasonic power 500 W) for 30 min. The foil was rinsed with water and ethanol in turn. After drying, the foil was placed in 0.1 M hydrochloric acid for 30 min to remove the surface oxide layer. After treatment, the foil was rinsed with deionized water and dried to obtain the pretreated iron foil.

[0077] (2) Preparation of self-supporting electrodes

[0078] The pretreated iron foil was placed in 0.01M NH3·H2O and ultrasonicated (ultrasonic power 80W) for 30 minutes and then allowed to stand for 180 minutes to etch its surface. After being taken out, it was rinsed with deionized water, dried, and heat treated at 250°C in Ar atmosphere for 60 minutes to obtain a self-supporting electrode with a metal oxide coating.

[0079] The prepared self-supporting electrode is used in a reaction device for water electrolysis.

[0080] Example 6

[0081] (1) Substrate pretreatment

[0082] A cobalt foil (1 cm in length, 1 cm in width, and 0.05 mm in thickness) was placed in a mixed solvent of acetone, ethanol, and water (the volume ratio of acetone, ethanol, and water was 1:1:1) and ultrasonicated (ultrasonic power 500 W) for 30 minutes. The foil was rinsed with water and ethanol in turn. After drying, the foil was placed in 0.1 M hydrochloric acid for 30 minutes to remove the surface oxide layer. After treatment, the foil was rinsed with deionized water and dried to obtain the pretreated cobalt foil.

[0083] (2) Preparation of self-supporting electrodes

[0084] The pretreated cobalt foil was placed in 0.1M NH3·H2O and ultrasonicated (ultrasonic power 80W) for 30 minutes and then allowed to stand for 180 minutes to etch its surface. After being taken out, it was rinsed with deionized water, dried, and heat treated at 250°C for 30 minutes in an Ar atmosphere to obtain a self-supporting electrode with a metal oxide coating.

[0085] The prepared self-supporting electrode is used in the reaction device of fuel cell.

[0086] Example 7

[0087] (1) Substrate pretreatment

[0088] A nickel foil (1 cm in length, 1 cm in width, and 0.04 mm in thickness) was placed in a mixed solvent of acetone, ethanol, and water (the volume ratio of acetone, ethanol, and water was 1:1:1) and ultrasonicated (ultrasonic power 500 W) for 30 min. The foil was rinsed with water and ethanol in turn. After drying, the foil was placed in 0.1 M hydrochloric acid for 30 min to remove the surface oxide layer. After treatment, the foil was rinsed with deionized water and dried to obtain a pretreated nickel foil.

[0089] (2) Preparation of self-supporting electrodes

[0090] The pretreated nickel foil was placed in 0.06M NH3·H2O and ultrasonicated (ultrasonic power 80W) for 30 minutes and then allowed to stand for 180 minutes to etch its surface. After being taken out, it was rinsed with deionized water, dried, and heat treated at 250°C in an Ar atmosphere for 30 minutes to obtain a self-supporting electrode with a metal oxide coating.

[0091] The prepared self-supporting electrode is used in the reaction device of the sensor.

[0092] Example 8

[0093] (1) Substrate pretreatment

[0094] The foam copper (1 cm in length, 1 cm in width, and 1 mm in thickness) was placed in a mixed solvent of acetone, ethanol and water (the volume ratio of acetone, ethanol and water was 1:1:1) and ultrasonicated (ultrasonic power 500 W) for 30 minutes, rinsed with water and ethanol in turn, and placed in 0.1 M hydrochloric acid for 30 minutes after drying to remove the surface oxide layer. After treatment, it was rinsed with deionized water and dried to obtain pretreated foam copper.

[0095] (2) Preparation of self-supporting electrodes

[0096] The pretreated copper foam was placed in 0.06M NH3·H2O and ultrasonicated (ultrasonic power 80W) for 30 minutes and then allowed to stand for 180 minutes to etch its surface. After being taken out, it was rinsed with deionized water, dried, and heat treated at 250°C for 30 minutes in an Ar atmosphere to obtain a self-supporting electrode with a metal oxide coating.

[0097] The prepared self-supporting electrode is used in a reaction device for electrochemical reduction of carbon dioxide.

[0098] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention shall be included in the protection scope of the present invention.

Claims

1. A self-supporting electrode, characterized in that: It includes a metal substrate and a metal oxide coating on the surface of the metal substrate.

2. The self-supporting electrode according to claim 1, characterized in that: The metal substrate is a metal foil or a foam metal, and the metal is at least one of Pt, Ir, Pd, Au, Ru, Rh, Ag, Cu, Fe, Co, Ni, and Mn.

3. The self-supporting electrode according to claim 1, characterized in that: The metal of the metal oxide coating is at least one of Pt, Ir, Pd, Au, Ru, Rh, Ag, Cu, Fe, Co, Ni, and Mn.

4. The self-supporting electrode according to claim 1, characterized in that: The thickness of the metal substrate is 0.02-10 mm; the thickness of the metal oxide coating is 1-10 μm.

5. A method for preparing a self-supporting electrode according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: (1) Pretreatment of metal substrate The metal substrate is placed in a mixed solvent of organic solvent and water and subjected to ultrasonic treatment for 10-60 minutes, and then rinsed with water and ethanol in turn, and after drying, placed in an acid solution for 15-60 minutes to remove the oxide layer on the surface; (2) Preparation of self-supporting electrodes The pretreated substrate is placed in an alkaline solution and treated physically at the same time, nucleation is induced on the surface of the substrate by physical and chemical means, and then allowed to stand for 0-240 minutes to allow the surface to be etched. After being taken out, it is rinsed with deionized water, dried, and heat treated at 150-750°C for 30-120 minutes to obtain a self-supporting electrode covered with a metal oxide coating.

6. The method for preparing the self-supporting electrode according to claim 5, characterized in that: In step (1), the organic solvent is at least one of methanol, ethanol, propanol, isopropanol, butanol, ethylene glycol, propylene glycol, ether, chloroform, cyclohexane, toluene and acetone; the volume ratio of the organic solvent to water in the mixed solvent of the organic solvent and water is 2:1-4:1; preferably, when the organic solvent is a mixture of acetone and ethanol, the volume ratio of acetone to ethanol is 1:1-3:

1.

7. The method for preparing a self-supporting bulk electrode according to claim 5, characterized in that: In step (1), the ultrasonic power is 400-600W; the acid is at least one of formic acid, acetic acid, phosphoric acid, hydrochloric acid and sulfuric acid; and the concentration of the acid solution is 0.01-10mol / L.

8. The method for preparing a self-supporting electrode according to claim 5, characterized in that: In step (2), the alkali is at least one of sodium hydroxide, potassium hydroxide, calcium hydroxide, lithium hydroxide, ammonia water, potassium carbonate, potassium bicarbonate, sodium carbonate, and sodium bicarbonate; and the concentration of the alkali solution is 0.01-10 mol / L.

9. The method for preparing a self-supporting electrode according to claim 5, characterized in that: In step (2), the physical means is at least one of laser, ultrasound, and microwave; when the physical means is ultrasound, the ultrasound time is 15-60 min and the ultrasound power is 60-90 W; the atmosphere of the heat treatment is at least one of helium, argon, nitrogen, hydrogen, air, and carbon monoxide.

10. Use of the self-supporting electrode according to claim 1 in water electrolysis, fuel cells, sensors, and electrochemical reduction of carbon dioxide.